A kind of organic silicon thermal conductive pad and preparation method thereof

By using dopamine-modified hydrogen-containing polysiloxane as a crosslinking agent and polydopamine coating in thermal conductivity gaskets, the problem of large interface thermal resistance of traditional thermal conductivity gaskets is solved, the thermal conductivity and adhesion are improved, and the thermal conductivity and adhesion are achieved. Silicone thermal gasket with low interface thermal resistance and high thermal conductivity.

CN117820705BActive Publication Date: 2024-11-12SHENZHEN JINLIAN TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311796283.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-11-12
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

Traditional thermal gaskets have poor heat transfer effects due to large interface thermal resistance, which limits their application.

Method used

Dopamine-modified hydrogen-containing polysiloxane is used as the crosslinking agent for the thermal gasket matrix, and the polydopamine coating is coated on the surface of the thermal gasket. By controlling the reaction temperature and the addition ratio, the compatibility and adhesion are improved and the adhesion is reduced. Interface thermal resistance.

Benefits of technology

It effectively improves the thermal conductivity coefficient of the thermal gasket, reduces the interface thermal resistance, and improves the reliability and heat transfer effect of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117820705B_ABST
    Figure CN117820705B_ABST
Patent Text Reader

Abstract

The present invention discloses a kind of organic silicon thermally conductive gasket, including a thermally conductive gasket substrate and a polydopamine coating coated on the surface of the thermally conductive gasket substrate, wherein the thermally conductive gasket substrate is mainly prepared by mixing the following raw materials: low-viscosity methyl vinyl silicone oil, dopamine-modified hydrogen-containing polysiloxane, aluminum oxide, platinum catalyst and inhibitor. Its preparation method is: first prepare a thermally conductive gasket base material, then vulcanize the base material to obtain a thermally conductive gasket base material, and then add the thermally conductive gasket base material to a dopamine-sodium hydroxide solution for immersion treatment to obtain an organic silicon thermally conductive gasket. The present invention introduces a polydopamine coating on the surface of the thermally conductive gasket after molding, and utilizes the chemical properties of more active groups such as amine groups and hydroxyls in the polydopamine coating, which can effectively reduce the contact thermal resistance between the thermally conductive gasket and the substrate, and the polydopamine coating can effectively improve the adhesion between the thermally conductive gasket and the substrate, thereby further improving the reliability of electronic components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of thermal conductive materials, and in particular relates to a low interface thermal resistance organic silicon thermal conductive pad and a preparation method thereof. Background Art

[0002] Thermally conductive silicone gasket is a type of thermal interface material, also known as thermally conductive rubber sheet, which is mainly used for heat transfer between heating elements (devices) and radiators. Thermally conductive silicone sheets have low hardness and can also provide protection for heating components and chips by buffering and reducing vibration.

[0003] With the development of high-heat-generating electronic industries such as automotive electronic systems and equipment, and high-power power supplies, it is discovered that heat dissipation and heat transfer in the future electronic industry will be problems that must be faced during the development process. Thermal grease, thermal gel, and thermal gaskets are the three most commonly used thermal conductive materials. Thermal gaskets have been most widely used due to their better use process and storage properties. However, in actual applications, traditional thermal gaskets often encounter the problem of large interface thermal resistance, resulting in poor heat transfer effect, which greatly limits the application of thermal gaskets. Therefore, it is urgent to develop a silicone thermal gasket with high thermal conductivity and low interface thermal resistance. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a low interface thermal resistance organic silicon thermal conductive gasket and a preparation method thereof.

[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0006] A silicone thermally conductive gasket comprises a thermally conductive gasket substrate and a polydopamine coating coated on the surface of the thermally conductive gasket substrate, wherein the thermally conductive gasket substrate is mainly prepared by mixing the following raw materials in parts by mass:

[0007]

[0008] The above-mentioned silicone thermal conductive gasket, preferably, the dopamine-modified hydrogenated polysiloxane is prepared by the following preparation method: dopamine compounds, hydrogenated siloxane and organic solvent are mixed, a catalyst is added dropwise, and the mixture is reacted at 40°C-120°C for 2-8h to obtain a preliminary sample, and the obtained preliminary sample is extracted and distilled under reduced pressure to obtain a light yellow viscous liquid, which is the dopamine-modified hydrogenated polysiloxane.

[0009] In the molecular design and preparation of dopamine-modified hydrogenated polysiloxane, the molecular weight of dopamine is introduced into the polysiloxane molecular chain through the hydroxyl group of the dopamine compound and the silicon hydrogen group of the hydrogenated polysiloxane under the action of an organic base catalyst, and quantitative control is performed by controlling the addition ratio and the reaction temperature.

[0010] In the above-mentioned silicone thermally conductive pad, preferably, the dopamine compound is selected from one or more combinations of dopamine, dopamine hydrochloride, N-biotin dopamine, 6-hydroxydopamine hydrobromide, 5-hydroxydopamine hydrochloride, dopamine 4-O-sulfate, and 6-hydroxydopamine hydrochloride;

[0011] The hydrogen-containing siloxane is one or more of terminal hydrogen-containing polysiloxane, side hydrogen-containing polysiloxane or terminal side hydrogen-containing polysiloxane, the viscosity of the hydrogen-containing siloxane is 10-1000mpa.s, and the mass ratio of hydrogen is 0.01%-0.8%;

[0012] The organic solvent is one or more of methanol, ethanol, butanol, isopropanol, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and ethyl acetate;

[0013] The catalyst is one or more of sodium ethoxide, potassium ethoxide, sodium methoxide, potassium methoxide, sodium tert-butoxide, and sodium isopropoxide.

[0014] In the above-mentioned silicone thermally conductive gasket, preferably, the mass ratio of the dopamine compound, the hydrogen-containing siloxane, and the catalyst is 1-100:1-50:0.1-0.5.

[0015] For the above-mentioned organosilicon thermally conductive gasket, preferably, the extraction is performed using one or more solvents selected from methanol, ethanol, n-butanol, and isopropanol.

[0016] In the above-mentioned organic silicon thermally conductive gasket, preferably, the vinyl content mass ratio of the low-viscosity methyl vinyl silicone oil is 0.05%-5%, and its viscosity is 50-2000 mPa·s.

[0017] In the above-mentioned organic silicon thermally conductive gasket, preferably, the platinum catalyst is a Custer platinum catalyst, wherein the platinum content is 1000-6000ppm;

[0018] The inhibitor is an alkynol catalyst, and the alkynol catalyst is selected from at least one of 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-hexynyl-1-cyclohexanol, and 3-phenyl-1-butyn-3-ol;

[0019] The alumina is spherical alumina with a particle size of 1-100 um.

[0020] The above-mentioned silicone thermally conductive gasket, preferably, the raw material of the thermally conductive gasket substrate also includes 0.1 to 10 parts of pigment, and the pigment is one of carbon black, iron oxide red and titanium dioxide.

[0021] In the above-mentioned silicone thermally conductive gasket, preferably, the thickness of the polydopamine coating is 10-100 um.

[0022] As a general inventive concept, the present invention also provides a method for preparing the above-mentioned silicone thermally conductive pad, comprising the following steps:

[0023] (1) low viscosity methyl vinyl silicone oil, dopamine modified hydrogenated polysiloxane and inhibitor are mixed and stirred evenly, then aluminum oxide and pigment are added and stirred evenly, and then platinum catalyst is added and stirred, and finally vacuum degassing is performed to obtain a base material;

[0024] (2) placing the base material in a molding vulcanizer for vulcanization treatment to obtain a thermally conductive gasket base;

[0025] (3) soaking the thermally conductive pad substrate obtained in step (2) in a dopamine-sodium hydroxide solution;

[0026] (4) The sample soaked in step (3) is cleaned and dried to obtain the organic silicone thermal conductive gasket.

[0027] In the above preparation method, preferably, in step (3), in the dopamine-sodium hydroxide solution, the mass ratio of dopamine to sodium hydroxide is 1:2-10, and the pH of the dopamine-sodium hydroxide solution is 7-10.

[0028] In the above preparation method, preferably, in step (3), the soaking treatment time is 1-5 hours and the soaking temperature is 30-100°C.

[0029] In the above preparation method, preferably, in step (2), the temperature of the vulcanization treatment is 120-180° C., and the vulcanization time is 10-30 min.

[0030] In the above-mentioned preparation method, preferably, in step (1), the specific process of preparing the base material is: placing low-viscosity methyl vinyl silicone oil, dopamine-modified hydrogenated polysiloxane, and inhibitor in a planetary mixer, stirring at 200-500 r / min for 10-20 min, then adding alumina and pigment, stirring at a speed of 500-1000 r / min for 1-2 h, and then continuing to add platinum catalyst, maintaining the stirring speed at 500-1000 r / min, continuing to stir for 5-10 min, and finally performing vacuum degassing treatment at a pressure of 0.08-0.1 MPa.

[0031] In the above preparation method, preferably, in step (4), the cleaning refers to cleaning the sample in one or more solvents selected from methanol, ethanol, butanol, isopropanol, acetone, and butanone, and the drying temperature is 60-120°C.

[0032] Compared with the prior art, the advantages of the present invention are:

[0033] (1) The present invention introduces a polydopamine coating on the surface of the thermally conductive gasket after molding, and utilizes the chemical properties of the relatively large number of active groups such as amine and hydroxyl groups in the polydopamine coating to effectively reduce the contact thermal resistance between the thermally conductive gasket and the substrate. At the same time, the polydopamine coating can effectively improve the adhesion between the thermally conductive gasket and the substrate, thereby further improving the reliability of electronic components.

[0034] (2) The present invention introduces dopamine-modified hydrogenated polysiloxane as a cross-linking agent for the thermally conductive gasket substrate, thereby introducing dopamine groups into the molecular chain segments of the thermally conductive gasket substrate, thereby effectively improving the compatibility between the thermally conductive gasket substrate and the polydopamine coating, and overcoming the weakness that the polar polydopamine coating is difficult to adhere to the non-polar polysiloxane surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the reaction mechanism of dopamine-modified hydrogen-containing polysiloxane in Example 1 of the present invention. DETAILED DESCRIPTION

[0036] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.

[0037] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0039] Embodiment 1:

[0040] The dopamine-modified hydrogen-containing polysiloxane used in this embodiment is obtained by the following preparation method:

[0041] (1) 50 g of dopamine, 25 g of terminal hydrogen-containing siloxane (viscosity 52 mPa.s, hydrogen content 0.18%) and 1000 mL of xylene were mixed, and then 0.2 g of sodium ethoxide was added dropwise for reaction. The reaction temperature was controlled at 100° C. and the reaction was carried out for 8 h to obtain a preliminary sample;

[0042] (2) Then, isopropanol solvent is used to extract the preliminary product obtained in step (1), and the solvent is removed by vacuum distillation to obtain a light yellow viscous liquid, thereby obtaining dopamine-modified hydrogen-containing polysiloxane. The reaction mechanism is as follows: Figure 1 shown.

[0043] The organic silicon thermally conductive gasket in this embodiment includes a thermally conductive gasket substrate and a polydopamine coating coated on the surface of the thermally conductive gasket substrate, wherein the thickness of the polydopamine coating is 45 um, and the thermally conductive gasket substrate is mainly prepared by mixing the following raw materials in parts by weight:

[0044] 15 parts of low-viscosity methyl vinyl silicone oil (vinyl content by mass ratio is 0.32%, viscosity is 100mpa.s),

[0045]

[0046] The method for preparing the organic silicon thermally conductive gasket in this embodiment comprises the following steps:

[0047] (1) Vinyl silicone oil, dopamine-modified hydrogenated polysiloxane, and inhibitor were sequentially added into a planetary mixer, stirred at 300 r / min for 15 min, then aluminum oxide and pigment were sequentially added, stirred at 800 r / min for 1.5 h, platinum catalyst was continuously added, the stirring speed was maintained at 800 r / min, stirring was continued for 10 min, and then vacuum degassing was performed at a pressure of 0.08 MPa to obtain a base material;

[0048] (2) placing the base material obtained in step (1) in a molding vulcanizer and vulcanizing at 150° C. for 20 min to obtain a thermally conductive gasket substrate;

[0049] (3) adding the thermally conductive pad substrate obtained in step (2) into a dopamine-sodium hydroxide solution and soaking it for 4 hours, wherein the soaking temperature is 50° C., the mass ratio of dopamine to sodium hydroxide in the dopamine-sodium hydroxide solution is 1:3, and the pH value is 8;

[0050] (4) The sample immersed in step (3) is cleaned with an ethanol solvent and dried at 100° C. to obtain a silicone thermally conductive gasket.

[0051] Embodiment 2:

[0052] The dopamine-modified hydrogen-containing polysiloxane used in this embodiment is obtained by the following preparation method:

[0053] (1) 30 g of dopamine, 25 g of side-group hydrogen-containing siloxane (viscosity 22 mPa.s, hydrogen content 0.5% by mass) and 800 mL of isopropanol were mixed, and then 0.1 g of sodium ethoxide was added dropwise for reaction. The reaction temperature was controlled at 100° C. and the reaction was carried out for 8 h to obtain a preliminary sample;

[0054] (2) extracting the preliminary product obtained in step (1) with n-butanol solvent and removing the solvent by vacuum distillation to obtain a light yellow viscous liquid, thereby obtaining dopamine-modified hydrogen-containing polysiloxane.

[0055] The organic silicon thermally conductive gasket in this embodiment includes a thermally conductive gasket substrate and a polydopamine coating coated on the surface of the thermally conductive gasket substrate, wherein the thickness of the polydopamine coating is 30 um, and the thermally conductive gasket substrate is mainly prepared by mixing the following raw materials in parts by weight:

[0056] 12 parts of low viscosity methyl vinyl silicone oil (vinyl content by mass ratio 0.76%, viscosity 200mpa.s),

[0057]

[0058] The preparation method of the organic silicon thermally conductive gasket in this embodiment is the same as that in embodiment 1.

[0059] Embodiment 3:

[0060] The dopamine-modified hydrogen-containing polysiloxane used in this embodiment is obtained by the following preparation method:

[0061] (1) 20 g of 5-hydroxydopamine hydrochloride, 15 g of side-group hydrogen-containing siloxane (viscosity 42 mPa.s, hydrogen content 0.28%) and 1000 mL of isopropanol were mixed, and then 0.1 g of sodium ethoxide was added dropwise to react. The reaction temperature was controlled at 100° C. and the reaction was carried out for 8 h to obtain a preliminary sample;

[0062] (2) extracting the preliminary sample obtained in step (1) with isopropanol solvent, and removing the solvent by vacuum distillation to obtain a light yellow viscous liquid, thereby obtaining dopamine-modified hydrogen-containing polysiloxane.

[0063] The organic silicon thermally conductive gasket in this embodiment includes a thermally conductive gasket substrate and a polydopamine coating coated on the surface of the thermally conductive gasket substrate, wherein the thickness of the polydopamine coating is 25 um, and the thermally conductive gasket substrate is mainly prepared by mixing the following raw materials in parts by weight:

[0064] 18 parts of methyl vinyl silicone oil (vinyl content by mass ratio is 0.76%, viscosity is 200mpa.s),

[0065]

[0066] The preparation method of the organic silicon thermally conductive gasket in this embodiment is the same as that in embodiment 1.

[0067] Comparative Example 1:

[0068] The commercially available HS-DRP-20 thermal conductive pad was selected as a reference in this comparative example.

[0069] Comparative Example 2:

[0070] The difference between this comparative example and Example 1 is that dopamine-modified hydrogen-containing polysiloxane is not introduced into the thermally conductive gasket substrate, and the dopamine-modified hydrogen-containing polysiloxane is replaced by an equal amount of terminal hydrogen-containing siloxane, and the polydopamine coating is applied under the same conditions.

[0071] Comparative Example 3:

[0072] The thermally conductive gasket of this comparative example is the thermally conductive gasket substrate in Example 1.

[0073] Table 1 Performance test results of the silicone thermally conductive pads of various embodiments and comparative examples

[0074]

[0075] From the comparison of the experimental data of the embodiment and the comparative example 1, it can be seen that the thermally conductive gasket of the present invention has the characteristics of low thermal resistance and high thermal conductivity compared with the thermally conductive gaskets available on the market. From the experimental data of embodiment 1 and comparative example 2, it can be seen that the use of dopamine-modified hydrogen-containing polysiloxane can effectively improve the compatibility between the thermally conductive gasket and the polydopamine coating, thereby reducing the contact thermal resistance of the thermally conductive gasket (0.96 down to 0.23℃*in2 / W). From the experimental data of embodiment 1 and comparative example 3, it can be seen that the use of polydopamine coating coating can effectively improve the adhesion between the thermally conductive gasket and the substrate, thereby effectively reducing the contact thermal resistance of the thermally conductive gasket (1.42 down to 0.23℃*in2 / W). In general, the present invention effectively improves the compatibility of the polydopamine coating and the thermally conductive gasket by modifying the hydrogen-containing polysiloxane with dopamine, and then introduces a stable polydopamine coating, and finally achieves the purpose of reducing the contact thermal resistance of the silicone thermally conductive gasket.

[0076] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A silicone thermally conductive pad, characterized in that: It comprises a thermally conductive gasket substrate and a polydopamine coating coated on the surface of the thermally conductive gasket substrate, wherein the thermally conductive gasket substrate is mainly prepared by mixing the following raw materials in parts by mass: 10-20 parts of low viscosity methyl vinyl silicone oil, 0.1 to 1 part of dopamine-modified hydrogen-containing polysiloxane, 1 to 100 parts of aluminum oxide, 0.1 to 10 parts of platinum catalyst, Inhibitor 0.1-10 parts; The dopamine-modified hydrogenated polysiloxane is prepared by the following preparation method: dopamine compounds, hydrogenated polysiloxane and organic solvent are mixed, a catalyst is added dropwise, and the mixture is reacted at 40°C-120°C for 2-8 hours to obtain a preliminary sample, and the obtained preliminary sample is extracted and distilled under reduced pressure to obtain a light yellow viscous liquid, which is the dopamine-modified hydrogenated polysiloxane.

2. The organic silicon thermally conductive pad according to claim 1, characterized in that: The dopamine compound is selected from one or more of dopamine, dopamine hydrochloride, N-biotin dopamine, 6-hydroxydopamine hydrobromide, 5-hydroxydopamine hydrochloride, dopamine 4-O-sulfate, and 6-hydroxydopamine hydrochloride; The hydrogen-containing polysiloxane is one or more of terminal hydrogen-containing polysiloxane, side hydrogen-containing polysiloxane or terminal side hydrogen-containing polysiloxane, the viscosity of the hydrogen-containing polysiloxane is 10-1000 mpa.s, and the mass ratio of hydrogen is 0.01%-0.8%; The organic solvent is one or more of toluene, xylene, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and ethyl acetate; The catalyst is one or more of sodium ethoxide, potassium ethoxide, sodium methoxide, potassium methoxide, sodium tert-butoxide, and sodium isopropoxide.

3. The organic silicon thermally conductive pad according to claim 1, characterized in that: The mass ratio of the dopamine compound, the hydrogen-containing polysiloxane and the catalyst is 1-100:1-50:0.1-0.

5.

4. The organic silicon thermally conductive pad according to any one of claims 1 to 3, characterized in that: The low-viscosity methyl vinyl silicone oil has a vinyl content of 0.05%-5% by mass and a viscosity of 50-2000 mPa•s; The platinum catalyst is a Custer platinum catalyst, wherein the platinum content is 1000-6000 ppm; The inhibitor is an alkynol catalyst, and the alkynol catalyst is selected from at least one of 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-hexynyl-1-cyclohexanol, and 3-phenyl-1-butyn-3-ol; The alumina is spherical alumina with a particle size of 1-100 um.

5. The organic silicon thermally conductive pad according to any one of claims 1 to 3, characterized in that: The raw materials of the thermal conductive pad substrate also include 0.1 to 10 parts of pigment, and the pigment is one of carbon black, iron oxide red and titanium dioxide.

6. The organic silicon thermally conductive pad according to any one of claims 1 to 3, characterized in that: The thickness of the polydopamine coating is 10-100 um.

7. A method for preparing the organic silicon thermally conductive gasket according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) low viscosity methyl vinyl silicone oil, dopamine modified hydrogenated polysiloxane and inhibitor are mixed and stirred evenly, then aluminum oxide and pigment are added and stirred evenly, and then platinum catalyst is added and stirred, and finally vacuum degassing is performed to obtain a base material; (2) placing the base material in a molding vulcanizer for vulcanization treatment to obtain a thermally conductive gasket base; (3) soaking the thermally conductive gasket substrate obtained in step (2) in a dopamine-sodium hydroxide solution; (4) The sample soaked in step (3) is cleaned and dried to obtain the organic silicone thermal conductive gasket.

8. The preparation method according to claim 7, characterized in that: In step (3), in the dopamine-sodium hydroxide solution, the mass ratio of dopamine to sodium hydroxide is 1:2-10, and the pH of the dopamine-sodium hydroxide solution is 8-10; The soaking time is 1-5 hours, and the soaking temperature is 30-100°C.

9. The preparation method according to claim 7, characterized in that: In step (2), the temperature of the vulcanization treatment is 120-180° C., and the vulcanization time is 10-30 min.