Titanium-containing composite material and preparation method and application thereof

By using titanium-containing composite materials as lithium extraction adsorbents, the problems of poor lithium extraction effect and complex operation in the existing technology are solved, and a method of efficiently and economically recovering lithium elements from waste lithium-ion batteries is realized, with excellent options sex and stability.

CN117839617BActive Publication Date: 2024-10-29JIANGSU HELPER FUNCTIONAL MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410079409.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-29
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

When existing technology recovers lithium from used lithium-ion batteries, the lithium extraction effect is poor, the operation is complex, and the cost is high, making it difficult to apply on a large scale.

Method used

Titanium-containing composite materials are used as highly selective lithium extraction adsorbents. The titanium source and lithium source are mixed with dopants by wet mixing and calcining. The acid solution is activated, and then reacted with polymer compounds to synthesize granular titanium-containing composite materials. Selective adsorption and separation of lithium from battery recycling fluid.

Benefits of technology

It achieves excellent selective adsorption performance for lithium ions, has good stability, can be recycled, has a simple and easy-to-control process, low equipment investment, low reagent cost, good product stability, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117839617B_ABST
    Figure CN117839617B_ABST
Patent Text Reader

Abstract

The present invention relates to a titanium-containing composite material and a preparation method and application thereof. The preparation method of the titanium-containing composite material comprises the following steps: mixing a lithium source, a titanium source and a dopant in a first solvent, preparing a titanium-lithium mixture by a hydrolysis reaction; calcining the titanium-lithium mixture to prepare a first intermediate; acid-activating the first intermediate to prepare a second intermediate; mixing the second intermediate, a polymer compound binder, bis(4-fluorosulfonylphenyl) ether, 4,4'-dibenzaldehyde and a catalyst in a second solvent, and granulating the mixture; the dopant is selected from a mixture of one or more selected from potassium salt, chitosan, clay mineral, silicon dioxide and a silane coupling agent. Using lithium as an adsorbent for the titanium-containing composite material can improve the adsorption efficiency and adsorption capacity of lithium ions, reduce titanium dissolution loss, and have good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adsorbents, and in particular to a titanium-containing composite material and a preparation method and application thereof. Background Art

[0002] Since the commercialization of lithium-ion batteries, they have been rapidly applied to various electronic mobile devices, such as mobile phones, computers, cars and some medical devices, due to their advantages such as light weight, high energy density and long cycle life. Compared with other cathode materials in lithium batteries, the theoretical energy density and actual energy density of ternary cathode materials are relatively high, and the cost is relatively low and the performance is stable. Therefore, ternary lithium-ion batteries will have more advantages in the future market.

[0003] With the increasing application of ternary lithium batteries, how to deal with waste lithium batteries has become an increasingly important issue. This is mainly because the toxic or carcinogenic chemicals contained in lithium-ion batteries are highly dangerous, especially the heavy metals contained in the positive electrode materials. If the waste batteries are not properly disposed of, heavy metals such as Ni, Co, and Mn will have an adverse effect on groundwater and soil. The random or direct disposal of waste lithium-ion batteries in landfills will lead to a series of safety problems such as explosions, electric shocks or fires. Therefore, recycling waste lithium-ion batteries and turning waste into treasure is of great and far-reaching significance. Especially the recycling of lithium elements. Recovering lithium from scrapped ternary lithium-ion batteries can not only greatly reduce the cost of lithium battery production, but also promote the lithium battery industry to form a "recycling" system that connects recycling and regeneration. The industry urgently needs to develop a solution for recycling lithium from waste ternary lithium batteries.

[0004] At present, a scheme has been reported that uses urea or urea-formaldehyde resin to thermally reduce the positive electrode material of ternary lithium-ion batteries to low-valent cobalt-nickel-manganese oxide, lithium oxide and lithium carbonate. The cobalt-nickel-manganese oxide, lithium oxide and lithium carbonate are leached with a CO2-saturated aqueous solution, and the lithium salts therein are dissolved in the leaching solution in the form of lithium bicarbonate and lithium carbonate, and then the manganese-based lithium ion sieve prepared from waste lithium-ion battery materials is used for adsorption and extraction of lithium. Or a scheme that uses high-temperature in-situ self-reduction magnetic separation of positive and negative mixed electrode sheets of waste lithium-ion batteries to separate the positive and negative electrode sheets in a first stage of water leaching, a second stage of alkaline leaching, and a third stage of water leaching to preferentially extract lithium elements, and a sulfuric acid roasting water leaching method for pre-extraction of lithium, which can selectively leach lithium. However, these schemes have poor lithium extraction effects, complex operations and high costs, and are difficult to apply on a large scale. Summary of the invention

[0005] Based on this, the present invention provides a titanium-containing composite material, which can be used as a highly selective lithium extraction adsorbent, has low titanium dissolution loss, is stable, and can be recycled.

[0006] The technical solution is as follows:

[0007] A method for preparing a titanium-containing composite material comprises the following steps:

[0008] Mixing a lithium source, a titanium source and a dopant in a first solvent to prepare a titanium-lithium mixture by hydrolysis reaction;

[0009] calcining the titanium-lithium mixture to prepare a first intermediate;

[0010] Performing acid activation treatment on the first intermediate to prepare a second intermediate;

[0011] The second intermediate, the polymer binder, bis(4-fluorosulfonylphenyl) ether, 4,4'-biphenylaldehyde and the catalyst are mixed in a second solvent and granulated;

[0012] The dopant is selected from a mixture of one or more of potassium salt, chitosan, clay mineral, silicon dioxide and silane coupling agent.

[0013] In one embodiment, the titanium source is selected from a mixture of one or more of titanium dioxide, tetraethyl titanate, tetrabutyl titanate, ilmenite, titanium isooctyloxide, titanium tetramethoxide and titanium acetylacetonate.

[0014] In one embodiment, the lithium source is selected from a mixture of one or more of lithium chloride, lithium sulfate, lithium hydroxide, lithium carbonate, lithium acetate, lithium dihydrogen phosphate and lithium oxalate.

[0015] In one embodiment, the molar ratio of the titanium source, the lithium source and the dopant is 1:(0.5-3):(0.1-2).

[0016] In one embodiment, the first solvent is selected from a mixture of one or more of methanol, ethanol, isopropanol, butanol and pentanol.

[0017] In one embodiment, the mass ratio of the first solvent to the titanium source is (2-8):1.

[0018] In one embodiment, the parameters of the hydrolysis reaction include:

[0019] The stirring speed is 280rpm~380rpm, the reaction temperature is 50℃~90℃, and the reaction time is 6h~24h.

[0020] In one embodiment, the calcination treatment includes a first calcination treatment and a second calcination treatment process, wherein the insulation temperature of the first calcination treatment is 400℃~800℃, and the insulation time is 6h~8h, and the insulation temperature of the second calcination treatment is 700℃~1200℃, and the insulation time is 2h~6h.

[0021] In one embodiment, the acid activation treatment time is 0.5h~5h.

[0022] In one embodiment, the acid used in the acid activation treatment is a mixture of one or more of hydrochloric acid, nitric acid and sulfuric acid.

[0023] In one embodiment, the mass ratio of the acid used in the acid activation treatment to the first intermediate is (7-10):1.

[0024] In one embodiment, the polymer compound binder is selected from a mixture of one or more of polyvinylidene fluoride, polyvinyl chloride, epoxy resin, polyethylene glycol, aramid fiber and sodium alginate.

[0025] In one embodiment, the second solvent is selected from a mixture of one or more of N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, ethanol and acetone.

[0026] In one embodiment, the mass ratio of the second intermediate, the organic solvent, the polymer compound, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde is 1:(5-15):(2-5):(3-6):(3-6).

[0027] In one embodiment, the mass ratio of the second intermediate, the organic solvent, the polymer compound, bis(4-fluorosulfonylphenyl) ether and 4,4'-bibenzaldehyde is 1:9:2:3:3.

[0028] In one embodiment, the catalyst is bis(triphenylphosphine)imide hydrogen fluoride, and the added amount is 3wt% to 6wt% of the 4,4'-biphenylaldehyde.

[0029] In one embodiment, the granulation treatment temperature is 80° C. to 100° C., the stirring speed is 280 rpm to 380 rpm, and the time is 0.5 h to 2 h.

[0030] In one embodiment, after the granulation step, the process further includes soaking the granules obtained by the granulation in methanol for 0.5 h to 2 h, and washing and drying the granules.

[0031] In one embodiment, the titanium-containing composite material is particles with a particle size of 0.2 mm to 0.6 mm.

[0032] The present invention also provides a titanium-containing composite material, which is prepared according to the preparation method of the titanium-containing composite material as described above.

[0033] The present invention also provides an adsorbent, which comprises the titanium-containing composite material as described above.

[0034] The present invention also provides a method for recovering lithium from waste lithium-ion batteries, comprising the following steps:

[0035] Dissolving metal ions in the discarded lithium-ion batteries through a leaching process to prepare a first mixed solution;

[0036] The adsorbent as described above is used as a lithium extraction adsorbent to extract lithium ions from the first mixed solution.

[0037] The present invention has at least the following beneficial effects:

[0038] The invention provides a method for preparing a titanium-containing composite material, wherein a titanium source and a lithium source are wet-mixed and calcined with a dopant, activated with an acid solution, and then reacted with a polymer compound to synthesize a granular titanium-containing composite material with a high titanium content. The granular titanium-containing composite material can be used as a lithium ion sieve powder and finished particles, has excellent performance in selectively adsorbing lithium ions, is suitable for selectively adsorbing and separating lithium from battery recovery liquid, has good stability, and can be recycled.

[0039] After testing, the titanium-containing composite material provided by the embodiment of the present invention is used as a lithium extraction adsorbent, and contains a variety of metal ions (Fe 3+ , Cu 2+ 、Ni 2+ 、Co 2+ 、Al 3+ and Li + ) in the presence of, the iron-loaded resin adsorption material of the present invention can adsorb a large amount of Li + , while for Fe 3+ , Cu 2+ 、Ni 2+ 、Co 2+ and Al 3+ The adsorption is poor, which reflects that the titanium-containing composite material of the present invention has high adsorption selectivity for lithium ions, low titanium dissolution loss, and less organic solvent dissolved into the solution. After being recycled for 5 times, the lithium ion adsorption capacity remains basically unchanged, showing excellent stability, and can be used as a stable and highly selective lithium extraction adsorbent.

[0040] In addition, the preparation method of the titanium-containing composite material provided by the present invention has simple and easy controllable process, simple operation, low equipment investment, low reagent cost, mild reaction conditions, green and environmental protection, high yield, pure product, easy product recovery, controllable quality and easy industrialization, and good environmental and economic effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 is a flow chart of the preparation of a titanium-containing composite material shown in one embodiment of the present invention;

[0042] Figure 2 is the XRD spectrum of the titanium-containing composite material obtained in Example 1;

[0043] Figure 3 is a SEM image of the titanium-containing composite material obtained in Example 1;

[0044] Figure 4 The titanium-containing composite material prepared in Example 1 is used as a lithium extraction adsorption material before and after adsorbing ternary lithium battery waste liquid;

[0045] Figure 5 The titanium-containing composite material prepared in Example 1 is used as a lithium extraction adsorption material and the Ti ion content in the solution is measured after five cycles. DETAILED DESCRIPTION

[0046] The present invention will be further described in detail below in conjunction with specific embodiments and accompanying drawings. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.

[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0048] Where “including,” “having,” and “comprising” are used herein, it is intended to cover a non-exclusive inclusion, and another component may also be added unless explicit limiting terms such as “only,” “consisting of,” etc. are used.

[0049] The words "preferably", "more preferably", "preferably", "better", etc. in the present invention refer to embodiments of the present invention that can provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the statement of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention. That is, in the present invention, "preferably", "more preferably", "preferably", "better", etc. are only used to describe implementation methods or examples with better effects, but do not constitute a limitation on the scope of protection of the present invention.

[0050] In the present invention, “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.

[0051] In the present invention, "at least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multilayer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present invention, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0052] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0053] If not otherwise specified, all steps of the present invention may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0054] In the present invention, "above" or "below" includes the number itself. For example, "below 1" includes 1.

[0055] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0056] Unless mentioned to the contrary, terms in the singular may include plural forms and should not be construed as being one in number.

[0057] The raw materials, reagents and materials used in the following specific embodiments are all commercially available products unless otherwise specified.

[0058] The main methods for recycling waste ternary lithium batteries include pyrometallurgy, hydrometallurgy, biometallurgy, mechanical grinding, etc. Pyrometallurgy is widely used because of its simple operation and high productivity. However, in order to pyrolyze the raw materials to form alloys, pyrometallurgy usually requires ultra-high temperatures. During the high-temperature smelting process, the negative electrode, electrolyte and plastic are oxidized to provide energy for the metallurgical process, but the waste gas generated at the same time requires additional purification equipment to suppress air pollution.

[0059] Hydrometallurgy generally recovers valuable metals from waste lithium-ion batteries through low-temperature leaching and subsequent separation and purification. The leachate rich in various precious metals is further regenerated into new positive electrode materials or high value-added products through various methods to maximize the recovery rate. The main disadvantages of the hydrometallurgical process include: (1) the steps are complicated, which increases the process cost and complexity; (2) a large amount of corrosive reagents are used during the operation, which not only complicates the wastewater treatment, but also increases the corresponding treatment costs.

[0060] Biometallurgy is also an effective technology for obtaining valuable metals from waste lithium-ion batteries. Waste lithium-ion batteries can be leached out of metals by producing acidic substances through bacteria or fungi. Compared with the expensive organic acids that directly leach metals, the inexpensive and environmentally friendly autotrophic bioleaching method can also achieve the recycling of waste lithium-ion batteries by generating organic acids. However, bioleaching faces huge challenges before industrialization: (1) It takes a long time to cultivate microorganisms, and (2) the effect of indirect acid leaching of metals is not ideal. Currently, hydrometallurgy accounts for the majority of lithium battery recycling. After the metal is dissolved in the leachate, multiple processes are required to recover different metals.

[0061] First, the leaching system is used to dissolve the metals in the waste lithium-ion batteries. However, in the subsequent separation, the properties of many metal ions are similar, making separation extremely difficult. It is often necessary to use other methods to separate various metals, which not only increases the complexity of the recycling process, but also increases the loss of valuable substances in the recycled raw materials. Usually, the main separation methods are precipitation, extraction, sol-gel method, adsorption method, etc. The core of the adsorption method is to prepare an adsorbent with high selectivity, large adsorption capacity and good cycle stability.

[0062] In recent years, the research reports on lithium extraction by adsorption method are mostly based on the use of inorganic adsorbents, mainly ion sieve oxides and aluminum adsorbents. Among them, ion sieve oxides include manganese ion sieves, titanium ion sieves and doped ion sieves. Manganese adsorbents are the research hotspot of lithium ion sieve adsorbents. They are spinel-type structures, mainly LiMn2O4, Li4Mn5O 12 , Li 1.6 Mn 1.6 O4, etc., lithium manganese oxide is acid-leached, Li + H +The expression of aluminum adsorbent is "LiCl·mAl(OH)3·nH2O" (Li / Al-LDHs), where LiCl is inserted into the amorphous Al(OH)3 interlayer and Li + Enter into the Al-O octahedral vacancy and deintercalate some Li + After that, the aluminum adsorbent has steric hindrance effect and memory effect, thereby selectively adsorbing Li + After saturation, it is washed with water without introducing other impurities, and the operating cost is low. However, this type of adsorbent is usually formed by co-precipitation of crystals aggregated into unstable particles, mostly in powder form, with poor mechanical strength and high dissolution rate. Therefore, it is usually necessary to granulate this type of adsorbent.

[0063] In view of the poor selective adsorption capacity of traditional titanium-based lithium extraction adsorbents for lithium and other impurity ions, it is difficult to achieve resin-based lithium extraction because the properties of multiple ions are similar, and the direct embedding method in the adsorbent technology has few active sites, and the resin hybridization reaction will lead to low aluminum loading capacity, which ultimately leads to problems such as low activity, exchange rate and lithium extraction capacity of the lithium extraction adsorbent, and it is urgently needed to be improved. In addition, during long-term operation, the titanium-based lithium extraction adsorbent will have defects such as physical wear, titanium dissolution, and poor selectivity for other cations, which affect its service life. The present invention provides a titanium-containing composite material, which can be used as a highly selective lithium extraction adsorbent, has low titanium dissolution, is stable, and can be recycled.

[0064] The technical solution is as follows:

[0065] A method for preparing a titanium-containing composite material comprises the following steps:

[0066] Mixing a lithium source, a titanium source and a dopant in a first solvent to prepare a titanium-lithium mixture by hydrolysis reaction;

[0067] calcining the titanium-lithium mixture to prepare a first intermediate;

[0068] Performing acid activation treatment on the first intermediate to prepare a second intermediate;

[0069] The second intermediate, the polymer binder, bis(4-fluorosulfonylphenyl) ether, 4,4'-biphenylaldehyde and the catalyst are mixed in a second solvent and granulated;

[0070] The dopant is selected from a mixture of one or more of potassium salt, chitosan, clay mineral, silicon dioxide and silane coupling agent.

[0071] The preparation method of the porous titanium composite material of the present invention is described in detail below in a step-by-step manner.

[0072] S100: mixing a lithium source, a titanium source and a dopant in a first solvent, and preparing a titanium-lithium mixture through a hydrolysis reaction.

[0073] In one embodiment, the titanium source is selected from a mixture of one or more of titanium dioxide, tetraethyl titanate, tetrabutyl titanate, ilmenite, titanium isooctyloxide, titanium tetramethoxide and titanium acetylacetonate.

[0074] In one embodiment, the lithium source is selected from a mixture of one or more of lithium chloride, lithium sulfate, lithium hydroxide, lithium carbonate, lithium acetate, lithium dihydrogen phosphate and lithium oxalate.

[0075] In the present invention, the dopant is selected from a mixture of one or more of potassium salt, chitosan, clay mineral, silicon dioxide and silane coupling agent. Among them, the potassium salt is selected from a mixture of one or more of potassium phosphate, potassium carbonate, potassium hydroxide, potassium dihydrogen phosphate and potassium sulfate, and the clay mineral is selected from a mixture of one or more of diatomaceous earth, perlite and kaolinite. The silane coupling agent is selected from aminosilane coupling.

[0076] In one embodiment, the molar ratio of the titanium source, the lithium source and the dopant is 1: (0.5-3): (0.1-2), including but not limited to 1: 0.5: 0.1, 1: 0.5: 0.5, 1: 0.5: 1, 1: 0.5: 1.5, 1: 0.5: 2, 1: 1: 0.1, 1: 1: 0.5, 1: 1: 1, 1: 1: 1.5, 1: 1: 2, 1: 1.5: 0.1, 1: 1 .5:0.5, 1:1.5:1, 1:1.5:1.5, 1:1.5:2, 1:2:0.1, 1:2:0.5, 1:2:1, 1:2:1.5, 1:2:2, 1:2.5:0.1, 1:2.5:0.5, 1:2.5:1, 1:2.5:1.5, 1:2.5:2, 1:3:0.1, 1:3:0.5, 1:3:1, 1:3:1.5, or 1:3:2.

[0077] In one embodiment, the first solvent is selected from a mixture of one or more of methanol, ethanol, isopropanol, butanol and pentanol.

[0078] In one embodiment, the mass ratio of the first solvent to the titanium source is (2-8):1, including but not limited to 2:1, 3:1, 4:1, 5:1, 6:1, 7:1 or 8:1.

[0079] In one embodiment, a lithium source, a titanium source and a dopant are mixed in a first solvent, and the parameters for preparing the titanium-lithium mixture include:

[0080] The stirring speed is 280 rpm~380 rpm, the temperature of the hydrolysis reaction is 50°C~90°C, and the time is 6h~24h.

[0081] The titanium source, lithium source and dopant are uniformly mixed through solvent, stirring and temperature treatment to form a uniform mixture, which is convenient for subsequent doping of dopant into titanium lithium compound.

[0082] S200: calcining the titanium-lithium mixture to prepare a first intermediate. Through the calcination, the dopant is doped into the crystal lattice of the titanium lithium compound.

[0083] In one embodiment, the calcination treatment includes a first calcination treatment and a second calcination treatment process. Further, the holding temperature of the first calcination treatment is 400°C to 800°C, including but not limited to 400°C, 450°C, 500°C, 520°C, 550°C, 560°C, 580°C, 600°C, 650°C, 700°C, 750°C or 800°C; the holding time of the first calcination treatment is 6h to 8h, including but not limited to 6h, 7h or 8h. The holding temperature of the second calcination treatment is 700°C to 1200°C, including but not limited to 700°C, 750°C, 800°C, 850°C, 900°C, 920°C, 950°C, 960°C, 980°C, 1000°C, 1050°C, 1100°C, 1150°C or 120°C; the holding time of the second calcination treatment is 2h to 6h, including but not limited to 2h, 3h, 4h, 5h or 6h. Further preferably, the temperature of the second calcination treatment is higher than the temperature of the first calcination treatment. Preferably, the holding temperature of the first calcination treatment is 500°C to 600°C, and the holding time is 6h to 8h; the holding temperature of the second calcination treatment is 700°C to 1000°C, and the holding time is 4h to 6h.

[0084] S300: performing acid activation treatment on the first intermediate to prepare a second intermediate. The lithium in the titanium lithium compound is removed by acid activation treatment, including partial removal or complete removal, so as to facilitate subsequent use as a lithium extraction adsorbent.

[0085] In one embodiment, the acid activation treatment time is 0.5h~5h, including but not limited to 0.5h, 1h, 2h, 3h, 4h or 5h.

[0086] In one embodiment, the acid used in the acid activation treatment is a mixture of one or more of hydrochloric acid, nitric acid and sulfuric acid. It can be understood that it is preferred to prepare the acid into a dilute acid for the acidification treatment, and the mass content of the acid in the dilute acid is 0.1% to 8%.

[0087] In one embodiment, the mass ratio of the acid used in the acid activation treatment to the first intermediate is (7-10):1, including but not limited to 10:1, 9:1, 8:1 or 7:1.

[0088] S400: The second intermediate, the polymer binder, bis(4-fluorosulfonylphenyl) ether, 4,4'-biphenylaldehyde and the catalyst are mixed in a second solvent and granulated.

[0089] In one embodiment, the polymer compound binder is selected from a mixture of one or more of polyvinylidene fluoride, polyvinyl chloride, epoxy resin, polyethylene glycol, aramid fiber and sodium alginate.

[0090] In one embodiment, the second solvent is selected from a mixture of one or more of N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, ethanol and acetone.

[0091] In one embodiment, the mass ratio of the second intermediate, the organic solvent, the polymer compound, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde is 1:(5-15):(2-5):(3-6):(3-6), including but not limited to 1:9:2:3:3, 1:10:2:3:3, 1:11:2:3:3, 1:12:2:3:3, 1:13:2:3:3, 1:14:2:3:3, 1:15:2:3:3, 1:9:5:3:3, 1:10:5:3:3, 1:11:5:3: 3, 1:12:5:3:3, 1:13:5:3:3, 1:14:5:3:3, 1:15:5:3:3, 1:9:2:6:3, 1:10:2:6:3, 1:11:2:6:3, 1:12:2:6:3, 1:13:2:6:3, 1:14:2:6:3, 1:15:2:6:3, 1:9:2:3:6, 1:10:2:3:6, 1:11:2:3:6, 1:12:2:3:6, 1:13:2:3:6, 1:14:2:3:6 or 1:15:2:3:3.

[0092] In one embodiment, the mass ratio of the second intermediate, the organic solvent, the polymer compound, bis(4-fluorosulfonylphenyl) ether and 4,4'-bibenzaldehyde is 1:9:2:3:3.

[0093] In one embodiment, the catalyst is bis(triphenylphosphine)imide hydrogen fluoride, and the added amount is 3wt% to 6wt% of the 4,4'-biphenylaldehyde.

[0094] In one embodiment, the granulation treatment temperature is 80° C. to 100° C., the stirring speed is 280 rpm to 380 rpm, and the time is 0.5 h to 2 h.

[0095] In one embodiment, after the granulation step, the process further includes soaking the granules obtained by the granulation in methanol for 0.5 h to 2 h, and washing and drying the granules.

[0096] Figure 1 It is a preparation flow chart of a titanium-containing composite material shown in one embodiment of the present invention.

[0097] In one embodiment, the titanium-containing composite material is particles with a particle size of 0.2 mm to 0.6 mm.

[0098] The present invention also provides a titanium-containing composite material, which is prepared according to the preparation method of the titanium-containing composite material as described above.

[0099] The present invention also provides an adsorbent, which comprises the titanium-containing composite material as described above.

[0100] The present invention also provides a method for recovering lithium from waste lithium-ion batteries, comprising the following steps:

[0101] Dissolving metal ions in the discarded lithium-ion batteries through a leaching process to prepare a first mixed solution;

[0102] The adsorbent as described above is used as a lithium extraction adsorbent to extract lithium ions from the first mixed solution.

[0103] The present invention is further described below with reference to specific embodiments and comparative examples.

[0104] Example 1

[0105] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0106] (a) Preparation of titanium-lithium mixture: tetrabutyl titanate, lithium acetate and potassium dihydrogen phosphate were weighed and added to anhydrous ethanol in a molar ratio of 1:0.5:0.2, wherein the mass ratio of tetrabutyl titanate to anhydrous ethanol was 1:5; the system was stirred at a stirring speed of 300 rpm, the temperature was raised to 80°C, and the reaction was refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; the compound was placed in a muffle furnace, calcined at 500°C for 6 hours and at 800°C for 6 hours; the obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0107] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 hours under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 hour, washed with pure water, and dried in an oven for 6 hours to obtain finished particles, which are recorded as product A and subsequently used as lithium extraction adsorption materials.

[0108] Figure 2 is the XRD spectrum of the titanium-containing composite material obtained in Example 1. Figure 2 It can be seen that part of the TiO2 lattice is occupied, and the composition of the titanium-containing composite material is Ti 0.784 O2. Figure 3 is a SEM image of the titanium-containing composite material obtained in Example 1. Figure 3 It can be seen that the titanium-containing composite material has a particle morphology.

[0109] Example 2

[0110] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0111] (a) Preparation of titanium-lithium mixture: titanium dioxide, lithium carbonate and potassium carbonate were weighed in a molar ratio of 1:1:0.3 and added to anhydrous ethanol, wherein the mass ratio of titanium dioxide to anhydrous ethanol was 1:5; the system was stirred at a stirring speed of 300 rpm, the temperature of the system was raised to 80°C, and the reaction was refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; the compound was placed in a muffle furnace, calcined at 500°C for 6 hours and at 800°C for 6 hours; the obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0112] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product B.

[0113] Example 3

[0114] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0115] (a) Preparation of titanium-lithium mixture: titanium dioxide, lithium carbonate and potassium carbonate were weighed in a molar ratio of 1:1:0.3 and added to anhydrous ethanol, wherein the mass ratio of titanium dioxide to anhydrous ethanol was 1:5; the mixture was stirred at a stirring speed of 300 rpm, the system was heated to 100°C, and refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; the mixture was placed in a muffle furnace, calcined at 500°C for 6 hours and at 800°C for 6 hours; the obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0116] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product C.

[0117] Example 4

[0118] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0119] (a) Preparation of titanium-lithium mixture: titanium dioxide, lithium carbonate and potassium carbonate were weighed in a molar ratio of 1:1:0.3 and added to anhydrous ethanol, wherein the mass ratio of titanium dioxide to anhydrous ethanol was 1:5; the system was stirred at a stirring speed of 300 rpm, the temperature was raised to 80°C, and the reaction was refluxed for 12 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; the compound was placed in a muffle furnace and calcined at 500°C for 6 hours and at 800°C for 6 hours. The obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture.

[0120] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product D.

[0121] Example 5

[0122] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0123] (a) Preparation of titanium-lithium mixture: Titanium dioxide, lithium carbonate and potassium carbonate were weighed in a molar ratio of 1:1:0.3 and added to anhydrous ethanol, wherein the mass ratio of titanium dioxide to anhydrous ethanol was 1:3; stirred at a stirring speed of 300 rpm, the system was heated to 100°C, and refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; placed in a muffle furnace, calcined at 500°C for 6 hours, and calcined at 800°C for 6 hours. The obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0124] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product E.

[0125] Example 6

[0126] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0127] (a) Preparation of titanium-lithium mixture: Tetrabutyl titanate, lithium carbonate and chitosan were weighed in a molar ratio of 1:0.5:0.2 and added to anhydrous ethanol, wherein the mass ratio of tetrabutyl titanate to anhydrous ethanol was 1:3. Stirring at a stirring speed of 300 rpm, the system was heated to 100°C and refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; placed in a muffle furnace, calcined at 500°C for 6 hours, and calcined at 800°C for 6 hours; the obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0128] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product F.

[0129] Example 7

[0130] This embodiment provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0131] (a) Preparation of titanium-lithium mixture: Weigh tetrabutyl titanate, lithium carbonate and silicon dioxide in a molar ratio of 1:1:0.3 and add them to anhydrous ethanol, wherein the mass ratio of tetrabutyl titanate to anhydrous ethanol is 1:3; stir at a stirring speed of 300 rpm, heat the system to 100°C, and reflux for 24 hours; dry the obtained compound at 80°C for 8 hours to obtain a powder. Put it into a muffle furnace, calcine at 500°C for 6 hours, and calcine at 800°C for 6 hours; wash and acidify the obtained powder in a 1wt% HCl solution, and dry it at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0132] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product G.

[0133] Comparative Example 1

[0134] This comparative example provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0135] (a) Preparation of titanium-lithium mixture: tetrabutyl titanate and lithium carbonate were weighed in a molar ratio of 1:1 and added to anhydrous ethanol, wherein the mass ratio of tetrabutyl titanate to anhydrous ethanol was 1:3; the mixture was stirred at a stirring speed of 300 rpm, the system was heated to 100°C, and refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; the obtained powder and NaCl were placed in a muffle furnace in a mass ratio of 7:1, and calcined at 500°C for 6 hours and at 800°C for 6 hours; the obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0136] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product H.

[0137] Comparative Example 2

[0138] This comparative example provides a titanium-containing composite material and a preparation method thereof, which are specifically as follows:

[0139] (a) Preparation of titanium-lithium mixture: tetrabutyl titanate and lithium carbonate were weighed and added to anhydrous ethanol in a molar ratio of 1:1, wherein the mass ratio of tetrabutyl titanate to anhydrous ethanol was 1:3; the mixture was stirred at a stirring speed of 300 rpm, the system was heated to 100°C, and refluxed for 24 hours; the obtained compound was dried at 80°C for 8 hours to obtain a powder; the obtained powder and CaCl2 were placed in a muffle furnace in a mass ratio of 10:1, and calcined at 500°C for 6 hours and at 800°C for 6 hours; the obtained powder was washed and acidified in a 1wt% HCl solution, and dried at 105°C for 8 hours to obtain a titanium-lithium mixture;

[0140] (b) In-situ granulation: The titanium-lithium mixture powder obtained in step (a), DMF, sodium alginate, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde are mixed in a mass ratio of 1:9:2:3:3, bis(triphenylphosphine)imide hydrogen fluoride is added as a catalyst, the temperature is raised to 80°C, and the mixture is stirred at a stirring speed of 300 rpm for 2 h under a mechanical stirrer. The obtained particles are then immersed in methanol for 1 h, washed with pure water, and dried in an oven for 6 h to obtain finished particles, which are recorded as product I.

[0141] The titanium-containing materials synthesized in Examples 1 to 6 and Comparative Examples 1 to 2 were tested:

[0142] (1) Take 10 mL of the titanium-containing composite material synthesized in Examples 1, 2, 3, 4, and 5 as a lithium extraction adsorption material and load it into a chromatography glass column with an inner diameter of 1.5 cm;

[0143] (2) Using self-simulated battery waste liquid as raw water, 5BV (1BV / h) was adsorbed and the lithium ion content in the waste liquid was determined. The results are shown in Table 1.

[0144] Table 1 Adsorption effect of titanium-containing composite materials on ternary lithium battery wastewater

[0145]

[0146] It can be seen from Table 1 above that, compared with Comparative Examples 1 and 2, the titanium-containing composite material synthesized in the embodiment of the present invention has better performance in selectively adsorbing lithium ions, among which the sample described in Example 1 has better measured effect.

[0147] After five cycles of 3BV pure water washing (6BV / h), 5BV 1wt% HCl desorption (2BV / h), and 1BV NaOH activation (2BV / h), the regeneration of the lithium adsorption material was repeated. The data of the re-adsorption are shown in Table 2:

[0148] Table 2 Re-adsorption effect of titanium-containing composite materials on ternary lithium battery waste liquid

[0149]

[0150] It can be seen from Table 2 above that, compared with Comparative Examples 1 and 2, the titanium-containing composite material synthesized in the embodiment of the present invention has better stability and can be recycled for multiple times.

[0151] Figure 4 This is a physical picture of the titanium-containing composite material prepared in Example 1 before and after absorbing ternary lithium battery waste liquid as a lithium extraction adsorption material. Figure 4 A in the middle is after adsorption. Figure 4 B is before adsorption. Figure 4 It can be seen that the material has obvious adsorption effect.

[0152] Figure 5 The titanium-containing composite material prepared in Example 1 is used as a lithium extraction adsorption material. After five cycles, the content of Ti ions in the solution is measured. Figure 5 It can be seen that the titanium dissolution rate of the titanium-containing composite material is low.

[0153] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0154] The above-described embodiments only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in detail, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present invention, several modifications and improvements can be made, which all belong to the protection scope of the present invention. It should be understood that the technical solutions obtained by ordinary technicians in this field through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the protection scope of the claims attached to the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the contents of the attached claims, and the description and drawings can be used to explain the contents of the claims.

Claims

1. A method for preparing a titanium-containing composite material, characterized in that: The steps include: Mixing a lithium source, a titanium source and a dopant in a first solvent to prepare a titanium-lithium mixture by hydrolysis reaction; calcining the titanium-lithium mixture to prepare a first intermediate; Performing acid activation treatment on the first intermediate to prepare a second intermediate; The second intermediate, the polymer binder, bis(4-fluorosulfonylphenyl) ether, 4,4'-biphenylaldehyde and the catalyst are mixed in a second solvent and granulated; The dopant is selected from a mixture of one or more of potassium salt, chitosan, clay mineral, silicon dioxide and silane coupling agent; The catalyst is bis(triphenylphosphine)imide hydrogen fluoride, and the added amount is 3wt% to 6wt% of the 4,4'-biphenylaldehyde; The granulation treatment is carried out at a temperature of 80° C. to 100° C., at a stirring speed of 280 rpm to 380 rpm, and for a time of 0.5 h to 2 h.

2. The method for preparing the titanium-containing composite material according to claim 1, characterized in that: The calcination treatment includes a first calcination treatment and a second calcination treatment process, wherein the insulation temperature of the first calcination treatment is 400°C~800°C, and the insulation time is 6h~8h, and the insulation temperature of the second calcination treatment is 700°C~1200°C, and the insulation time is 2h~6h.

3. The method for preparing the titanium-containing composite material according to claim 1, characterized in that: Satisfy at least one of the following (1) to (3): (1) The titanium source is selected from a mixture of one or more of titanium dioxide, tetraethyl titanate, tetrabutyl titanate, ilmenite, titanium isooctyloxide, titanium tetramethoxide and titanium acetylacetonate; (2) The lithium source is selected from a mixture of one or more of lithium chloride, lithium sulfate, lithium hydroxide, lithium carbonate, lithium acetate, lithium dihydrogen phosphate and lithium oxalate; (3) The molar ratio of the titanium source, the lithium source and the dopant is 1:(0.5-3):(0.1-2).

4. The method for preparing the titanium-containing composite material according to claim 1, characterized in that: Satisfy at least one of the following (1) to (3): (1) The first solvent is selected from a mixture of one or more of methanol, ethanol, isopropanol, butanol and pentanol; (2) The mass ratio of the first solvent to the titanium source is (2-8):1; (3) The parameters of the hydrolysis reaction include: The stirring speed is 280rpm~380rpm, the reaction temperature is 50℃~90℃, and the reaction time is 6h~24h.

5. The method for preparing the titanium-containing composite material according to claim 1, characterized in that: The acid activation treatment satisfies at least one of the following (1) to (3): (1) The acid activation treatment time is 0.5h~5h; (2) The acid used in the acid activation treatment is a mixture of one or more of hydrochloric acid, nitric acid and sulfuric acid; (3) The mass ratio of the acid used in the acid activation treatment to the first intermediate is (7-10):

1.

6. The method for preparing the titanium-containing composite material according to claim 1, characterized in that: The mass ratio of the second intermediate, the organic solvent, the polymer compound, bis(4-fluorosulfonylphenyl) ether and 4,4'-biphenylaldehyde is 1:(5-15):(2-5):(3-6):(3-6).

7. The method for preparing the titanium-containing composite material according to claim 1, characterized in that: The granulation process satisfies at least one of the following (1) to (2): (1) The second solvent is selected from a mixture of one or more of N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, ethanol and acetone; (2) The polymer compound binder is selected from a mixture of one or more of polyvinylidene fluoride, polyvinyl chloride, epoxy resin, polyethylene glycol, aramid fiber and sodium alginate.

8. The method for preparing a titanium-containing composite material according to any one of claims 1 to 7, characterized in that: After the granulation step, the method further includes soaking the granules obtained by the granulation in methanol for 0.5 h to 2 h, and washing and drying the granules.

9. The method for preparing a titanium-containing composite material according to any one of claims 1 to 7, characterized in that: The titanium-containing composite material is in the form of particles with a particle size of 0.2 mm to 0.6 mm.

10. A titanium-containing composite material, characterized in that: The titanium-containing composite material is prepared according to the preparation method of any one of claims 1 to 9.

11. An adsorbent, characterized in that: The titanium-containing composite material comprises the titanium-containing composite material according to claim 10.

12. A method for recovering lithium from waste lithium-ion batteries, characterized in that: The steps include: Dissolving metal ions in the discarded lithium-ion batteries through a leaching process to prepare a first mixed solution; The adsorbent according to claim 11 is used as a lithium extraction adsorbent to extract lithium ions from the first mixed solution.

Citation Information

Patent Citations

  • Preparation method of doped Li4Ti5O12 anode material

    CN104810515A

  • Lithium ion sieve adsorbent and preparation method and application thereof

    CN112844298A