A high-strength solder based on SnBi alloy
By combining tin bismuth alloy powder with loading metal single atom graphene, the thermal conductivity and mechanical strength of SnBi alloy solder are improved, the problem of insufficient toughness of existing solder is solved, the low-temperature packaging needs of electronic components is met and the low-temperature packaging is reduced. cost.
Patent Information
- Application Number
- CN202410101643.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-25
AI Technical Summary
The existing Sn42Bi58 alloy solder has insufficient toughness during the welding process, which cannot meet the actual performance requirements of diversified electronic components and has adverse thermal impacts on electronic components.
Using high-strength solder based on SnBi alloy, the content of single-atom graphene of the loading metal is 0.05-2.0 wt% to improve the thermal conductivity, mechanical strength and resistance of the solder. Impact toughness.
It effectively solves the tough brittle performance defects of tin bismuth alloy, improves the thermal conductivity and mechanical strength of the solder, meets the low-temperature packaging needs of precision electronic devices, and reduces the overall cost.
Smart Images

Figure BDA0004680408600000121 
Figure BDA0004680408600000131
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of low-temperature solders, and in particular to a high-strength solder based on SnBi alloy. Background Art
[0002] With the development of 5G technology and the advancement of electronic manufacturing technology, the demand for miniaturization, high density, and high integration of integrated circuit boards has become higher and higher, which puts higher requirements on packaging materials. The welding process of packaging materials will cause adverse thermal effects on electronic components. The higher the welding temperature of the packaging materials, the greater the thermal impact on electronic components. In order to reduce the adverse thermal effects on electronic components during the welding process, the eutectic point of the packaging materials needs to be low, that is, the concept of low-temperature packaging materials.
[0003] Commonly used low-temperature packaging materials in the prior art include Bi-containing alloy solders with bismuth content >40%. At present, the Sn42Bi58 alloy solder has the largest market share among Bi-containing alloy solders. Its eutectic point is 138°C, which can well meet the low-temperature packaging needs of electronic components and is suitable for the low-temperature packaging needs of electronic components with special low-temperature packaging requirements such as the most cutting-edge flexible solar panels, thermal sensitive components, and solar laminated battery structure devices. However, the Sn42Bi58 alloy solder also has the disadvantage of insufficient toughness and often cannot meet the actual performance requirements of diversified electronic components. In response to the toughness defects in the above-mentioned related technologies, the applicant provides a high-strength solder based on SnBi alloy. Summary of the invention
[0004] In order to solve the above technical problems, the present application provides a high-strength solder based on SnBi alloy.
[0005] The present application provides a high-strength solder based on SnBi alloy, which is realized by the following technical solutions:
[0006] A high-strength solder based on SnBi alloy is mainly made of tin-bismuth alloy powder and metal single-atom graphene loaded. The content of metal single-atom graphene loaded in the high-strength solder based on SnBi alloy is 0.05-2.0wt%; the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene loaded include at least Sn and Bi.
[0007] The present application uses metal-loaded single-atom graphene to effectively solve the compatibility problem between graphene materials and tin-bismuth alloy powders, making up for the toughness and brittleness defects of the original tin-bismuth alloy, and giving the prepared tin-bismuth SnBi alloy solder good thermal conductivity, mechanical strength and impact toughness, which can meet the low-temperature packaging requirements of precision electronic devices.
[0008] Preferably, the eutectic point of the Sn-Bi alloy powder is 138-145°C.
[0009] Preferably, the tin-bismuth alloy powder is at least one of tin-42-bismuth-58 alloy powder, tin-57-bismuth-43 alloy powder, tin-52-silver-32-bismuth-16 alloy powder, and tin-42-silver-35-bismuth-23 alloy powder; the eutectic point of the tin-42-bismuth-58 alloy powder is 138°C, the eutectic point of the tin-57-bismuth-43 alloy powder is 139°C, the eutectic point of the tin-52-silver-32-bismuth-16 alloy powder is 138°C, and the eutectic point of the tin-42-silver-35-bismuth-23 alloy powder is 141°C.
[0010] Preferably, when the tin-bismuth alloy powder is tin-42-bismuth-58 alloy powder, the metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 42:58; when the tin-bismuth alloy powder is tin-57-bismuth-43 alloy powder, the metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 57:43; when the tin-bismuth alloy powder is When the tin-bismuth alloy powder is tin-52-silver-32-bismuth-16 alloy powder, the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 52:32:16; when the tin-bismuth alloy powder is tin-42-silver-35-bismuth-23 alloy powder, the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 42:35:23.
[0011] By adopting the above technical solution, the low-temperature packaging requirements of precision electronic devices can be met while solving the toughness and brittleness defects of the original tin-bismuth alloy and the compatibility problem of graphene materials and tin-bismuth alloy powder, giving the prepared tin-bismuth SnBi alloy solder good thermal conductivity, mechanical strength and impact toughness.
[0012] Preferably, the tin-bismuth alloy powder is tin-57-bismuth-43 alloy powder, and the eutectic point of the tin-57-bismuth-43 alloy powder is 139° C.; the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 57:43.
[0013] By adopting the above technical solution, the low-temperature packaging requirements of precision electronic devices can be met while reducing the overall cost.
[0014] Preferably, the content of the metal-loaded single-atom graphene is 0.2-0.8wt%; and the mass ratio of the metal single atom loaded on the surface of the graphene carrier to the graphene carrier in the metal-loaded single-atom graphene is 1:(10-50).
[0015] Preferably, the content of the metal-loaded single-atom graphene is 0.4-0.5wt%; and the mass ratio of the metal single atom loaded on the surface of the graphene carrier to the graphene carrier in the metal-loaded single-atom graphene is 1:(20-25).
[0016] By adopting the above technical solution, the low-temperature packaging requirements of precision electronic devices can be met while reducing the overall cost.
[0017] Preferably, the number of layers of the graphene carrier in the metal-loaded single-atom graphene is less than 10, the sheet diameter is less than 5 μm, the thickness is less than 5 nm, and the specific surface area is 100-1000 m 2 / g.
[0018] By adopting the above technical solution, the quality stability of the prepared tin-bismuth SnBi alloy solder is guaranteed.
[0019] Preferably, the tin-bismuth alloy powder is made of the following alloy elements: 42-45% bismuth Bi, 0.05-0.2% tungsten W, 0.4-0.8% indium In, 0.05-0.25% cobalt Co, 0.10-0.25% cerium Ce, and the balance is tin Sn; the eutectic point of the tin-bismuth alloy powder is 140-145°C; the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene loaded include at least Sn, Bi, and In.
[0020] By adopting the above technical solution, the good thermal conductivity, mechanical strength and impact toughness of the prepared tin-bismuth SnBi alloy solder can be further improved, which can better meet the low-temperature packaging requirements of precision electronic devices.
[0021] Preferably, the method for preparing a high-strength solder based on SnBi alloy comprises the following steps: melting the tin-bismuth alloy powder into a liquid state, adding the loaded metal single-atom graphene, stirring for 10-30 minutes under nitrogen protection, and cooling and molding to obtain the high-strength solder based on SnBi alloy.
[0022] The metal single-atom graphene and tin-bismuth alloy powder loaded in the present application can be directly prepared by the traditional molten alloy production process. The preparation method provided in the present application is simple and has low operating difficulty compared to the powder metallurgy process, which is convenient for mass production.
[0023] In summary, this application has the following advantages:
[0024] 1. This application uses metal-loaded single-atom graphene to effectively solve the compatibility problem between graphene materials and tin-bismuth alloy powders, making up for the toughness and brittleness defects of the original tin-bismuth alloy, and giving the prepared tin-bismuth SnBi alloy solder good thermal conductivity, mechanical strength and impact toughness, which can meet the low-temperature packaging requirements of precision electronic devices.
[0025] 2. The metal-loaded single-atom graphene and tin-bismuth alloy powder in the present application can be directly prepared by conventional molten alloy production processes. The preparation method provided in the present application is relatively simple and has low operating difficulty compared to the powder metallurgy process, and is convenient for mass production. DETAILED DESCRIPTION
[0026] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with the examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the invention. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve.
[0027] Example
[0028] A high-strength solder based on SnBi alloy is mainly made of tin-bismuth alloy powder and metal single-atom graphene, the eutectic point of the tin-bismuth alloy powder is 138-145° C. The metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene at least include Sn and Bi.
[0029] Preferably, the tin-bismuth alloy powder is at least one of tin-42-bismuth-58 alloy powder, tin-57-bismuth-43 alloy powder, tin-52-silver-32-bismuth-16 alloy powder, and tin-42-silver-35-bismuth-23 alloy powder.
[0030] Among them, the eutectic point of tin-42-bismuth-58 alloy powder is 138°C, the eutectic point of tin-57-bismuth-43 alloy powder is 139°C, the eutectic point of tin-52-silver-32-bismuth-16 alloy powder is 138°C, and the eutectic point of tin-42-silver-35-bismuth-23 alloy powder is 141°C.
[0031] When the tin-bismuth alloy powder is tin-42-bismuth-58 alloy powder, the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 42:58.
[0032] When the tin-bismuth alloy powder is tin-57-bismuth-43 alloy powder, the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 57:43, which has better comprehensive performance and is the most economical solution.
[0033] When the tin-bismuth alloy powder is a tin-52-silver-32-bismuth-16 alloy powder, the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 52:32:16.
[0034] When the tin-bismuth alloy powder is a tin-42-silver-35-bismuth-23 alloy powder, the metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 42:35:23.
[0035] In order to further improve the overall comprehensive performance of the solder, the tin-bismuth alloy powder is made of the following alloy elements: 42-45% bismuth Bi, 0.05-0.2% tungsten W, 0.4-0.8% indium In, 0.05-0.25% cobalt Co, 0.10-0.25% cerium Ce, and the balance is tin Sn; the eutectic point of the tin-bismuth alloy powder is 140-145°C; the metal single atoms loaded on the surface of the graphene carrier in the metal single atom graphene at least include Sn, Bi, and In.
[0036] Preferably, the tin-bismuth alloy powder is made of the following alloy elements: 43% bismuth Bi, 0.06% tungsten W, 0.5% indium In, 0.12% cobalt Co, 0.15% cerium Ce, and the balance is tin Sn. The eutectic point of the tin-bismuth alloy powder is 140.8°C. The metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene at least include Sn, Bi, and In. Preferably, the metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene are Sn, Bi, and In in a mass ratio of 113:86:1.
[0037] The content of metal single-atom graphene loaded in the high-strength solder based on SnBi alloy is 0.05-2.0wt%.
[0038] Preferably, the content of metal-loaded single-atom graphene is 0.2-0.8 wt %.
[0039] Further preferably, the content of metal single-atom graphene is 0.4-0.5 wt %.
[0040] The mass ratio of the metal single atom loaded on the surface of the graphene carrier in the metal single atom graphene loaded with metal is 1:(10-50). Preferably, the mass ratio of the metal single atom loaded on the surface of the graphene carrier in the metal single atom graphene loaded with metal is 1:(20-25). The preferred scheme of the graphene carrier is as follows: the number of layers of the graphene carrier in the metal single atom graphene loaded with metal is <10, the sheet diameter is <5μm, the thickness is <5nm, and the specific surface area is 100-1000m 2 / g.
[0041] Example 1: A high-strength solder based on SnBi alloy is made of 99.6wt% of Sn-42-Bi-58 alloy powder (Wuxi Fanchuan Tin Industry Co., Ltd.) and 0.4wt% of loaded metal single atom graphene. The metal single atoms loaded on the surface of the graphene carrier in the loaded metal single atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 42:58. The mass ratio of the metal single atoms loaded on the surface of the graphene carrier in the loaded metal single atom graphene to the graphene carrier is 1:20. The graphene carrier is a highly conductive graphene TNHRGO (prepared by plasma method) of Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences, with a layer number of <10, a sheet diameter of 0.06-0.12μm, a thickness of <5nm, and a specific surface area of 150-200m 2 / g, ash content (ASH) <1wt%.
[0042] A method for preparing a high-strength solder based on SnBi alloy comprises the following steps:
[0043] S1, Preparation of metal-loaded single-atom graphene:
[0044] S1.1, construct defect points on the graphene carrier: select a customized quartz glass container with a volume of 5 liters (the quartz glass container has a jacket layer, and the jacket layer can be passed into the heat exchange medium to control the material temperature). After cleaning, pass ice water into the jacket layer of the container for heat exchange, then add 846.4g of concentrated sulfuric acid and 10g of sodium nitrate, stir at 300rpm for 10min, add 20g of highly conductive graphene TNHRGO, adjust the speed to 500rpm and stir for 150min, then adjust the flow rate of ice water input into the jacket layer of the container to control the material temperature in the container between 10-15℃, and maintain the rotation speed. 60 g of potassium permanganate powder was added to a quartz glass container at a speed of 1 g / 10 s at 500 rpm. After the addition of potassium permanganate powder, stirring was continued at 500 rpm for 10 min. Then, 37°C constant temperature exchange water was introduced into the jacket layer of the container to control the material temperature in the container at 35-35.5°C. Stirring was continued at 500 rpm for 120 min. Then, 800 mL of distilled water was added to the container at a speed of 200 rpm using a glass cup. After the addition of distilled water, stirring was continued at 200 rpm for 10 min. Then, 99°C was introduced into the jacket layer of the container. ℃ hot water heat exchange, so that the liquid material in the container is heated to 98-98.5 and kept warm for 20 minutes, then 37℃ constant temperature hot water is introduced into the jacket layer of the container, and 3.0L distilled water and 50mL hydrogen peroxide (10mol / L) are added to the date, the speed is adjusted to 800rpm and mechanical stirring is performed for 60min, stirring is stopped and the etching reaction is allowed to stand at room temperature for 12h, and 2L of supernatant is taken out with a dropper, and 2L of distilled water and 5mL hydrogen peroxide (10mol / L) are added, and stirring is performed at 800rpm for 60min, and stirring is stopped and the etching reaction is allowed to stand at room temperature for 12h. The second time, the supernatant is taken out with a dropper, and 2L of distilled water and 5mL hydrogen peroxide (10mol / L) are added, and stirring is performed at 800rpm for 60min, and stirring is stopped and the etching reaction is allowed to stand at room temperature for 12h. 2L of supernatant was drawn with a pipette, and then 2L of distilled water and 5mL of hydrogen peroxide (10mol / L) were added, stirred at 800rpm for 60min, and then the stirring was stopped and the etching reaction was carried out at room temperature for 12h. For the third time, 2L of supernatant was drawn with a pipette, and then 2L of distilled water and 5mL of hydrogen peroxide (10mol / L) were added, stirred at 800rpm for 60min, and then the stirring was stopped and the etching reaction was carried out at room temperature for 12h. After the slow etching, the obtained graphene paste was washed by centrifugation with distilled water until it was neutral, and finally placed in a vacuum dryer at 50°C for 48h to obtain a graphene carrier with surface defect points;
[0045] S1.2, weigh 11.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 11.26g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 10.15g of 1,10-phenanthroline, 8.58g of 2-methylimidazole, and 7.24g of glucose into a 1L clean glass beaker, add 800mL of distilled water and 200mL of ethanol into the glass beaker, and ultrasonicate at an ultrasonic frequency of 80kHz and an ultrasonic power of 800W until the metal is completely dissolved. The precursor solution was prepared, and then the graphene carrier with surface-defective sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the temperature at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-defective sites was 1:20, that is, 20 g of the graphene carrier with surface-defective sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C and then dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm;
[0046] S1.3, the obtained particle size D 50 =100-200nm solid powder was heated to 240℃ at 4℃ and kept for 15min, then heated to 540℃ at 6℃ and kept for 1h, then heated to 780℃ at 6℃ / min and kept for 1h under the condition of 5% v nitrogen-argon mixed gas (nitrogen:argon=95:5), and then cooled to room temperature naturally. The solid was taken out and ball-milled in a planetary ball mill at 100rpm for 60min to obtain a particle size D 50 = 100-200nm metal-loaded single-atom graphene;
[0047] S2, melt the precisely measured Sn-42-Bi-58 alloy powder into liquid state, add the precisely measured metal-loaded single-atom graphene prepared in S1.3, stir for 15 minutes under nitrogen protection, and cool and shape to obtain the high-strength solder of SnBi alloy.
[0048] The difference between Example 2 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.95wt% of Sn-42-Bi-58 alloy powder and 0.05wt% of loaded metal single-atom graphene.
[0049] The difference between Example 3 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.2wt% of Sn-42-Bi-58 alloy powder and 0.8wt% of loaded metal single-atom graphene.
[0050] The difference between Example 4 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99wt% Sn-42-Bi-58 alloy powder and 1wt% loaded metal single atom graphene.
[0051] The difference between Example 5 and Example 1 is that a high-strength solder based on SnBi alloy is made of 98wt% Sn-42-Bi-58 alloy powder and 2wt% loaded metal single-atom graphene.
[0052] The difference between Example 6 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.5wt% of Sn-57-Bi-43 alloy powder (customized by Hebei Yirui Alloy Welding Material Co., Ltd.) and 0.5wt% of loaded metal single-atom graphene. The metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 57:43. The mass ratio of the metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene to the graphene carrier is 1:20.
[0053] A method for preparing a high-strength solder based on SnBi alloy comprises the following steps:
[0054] S1, Preparation of metal-loaded single-atom graphene:
[0055] S1.1 is the same as S1.1 in Example 1, firstly preparing a graphene carrier with surface defect points;
[0056] S1.2, weigh 15.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 8.35g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 9.32g of 1,10-phenanthroline, 8.10g of 2-methylimidazole, and 6.78g of glucose into a 1L clean glass beaker, add 800mL of distilled water and 200mL of ethanol into the glass beaker, and ultrasonicate at an ultrasonic frequency of 80kHz and an ultrasonic power of 800W until the metal precursor is completely dissolved. The solution was prepared, and then the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the temperature at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:20, that is, 20 g of the graphene carrier with surface-trapped defect sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size of D 50 = Solid powder of 100-200nm;
[0057] S1.3, the obtained particle size D 50 =100-200nm solid powder was heated to 250℃ at 4℃ and kept for 20min in 8% v nitrogen-argon mixed gas (nitrogen:argon=92:8), then heated to 550℃ at 6℃ and kept for 1h, then heated to 800℃ at 6℃ / min and kept for 1h, then cooled to room temperature naturally, and the solid was taken out and ball-milled in a planetary ball mill at 100rpm for 60min to obtain a particle size D 50 = 100-200nm metal-loaded single-atom graphene;
[0058] S2, melt the precisely measured Sn-57-Bi-43 alloy powder into liquid state, add the precisely measured metal-loaded single-atom graphene prepared in S1.3, stir for 15 minutes under nitrogen protection, and cool and shape to obtain the high-strength solder of SnBi alloy.
[0059] The difference between Example 7 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.5wt% of Sn-52-Ag-32-Bi-16 alloy powder (customized by Nangong Dinghong Metal Materials Co., Ltd.) and 0.5wt% of loaded metal single-atom graphene. The metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 52:32:16. The mass ratio of the metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene to the graphene carrier is 1:20.
[0060] A method for preparing a high-strength solder based on SnBi alloy comprises the following steps:
[0061] S1, Preparation of metal-loaded single-atom graphene:
[0062] S1.1 is the same as S1.1 in Example 1, firstly preparing a graphene carrier with surface defect points;
[0063] S1.2, weigh 13.88g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 3.1g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 5.04g of silver nitrate, 8.48g of 1,10-phenanthroline, 7.84g of glucose and add them into a 1L clean glass beaker, add 800mL of distilled water and 200mL of ethanol into the glass beaker, and ultrasonicate at an ultrasonic frequency of 80kHz and an ultrasonic power of 800W until the metal precursor solution is completely dissolved, and then Then, the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the speed at 500 rpm. The mass ratio of the total mass of the tin single atom, the silver single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:20, that is, 20 g of the graphene carrier with surface-trapped defect sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C and then dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm;
[0064] S1.3, the obtained particle size D 50 =100-200nm solid powder was heated to 220℃ at 4℃ and kept for 20min, then heated to 520℃ at 6℃ / min and kept for 1h, then heated to 750℃ at 6℃ / min and kept for 1h, then cooled to room temperature naturally, and the solid was taken out and ball milled at 100rpm for 60min in a planetary ball mill to obtain a particle size D 50 = 100-200nm metal-loaded single-atom graphene;
[0065] S2, after the precisely measured Sn-52-Ag-32-Bismuth-16 alloy powder is melted into liquid, the precisely measured metal-loaded single-atom graphene prepared in S1.3 is added and stirred for 20 minutes under nitrogen protection, and then cooled and formed to obtain the high-strength solder of SnBi alloy.
[0066] The difference between Example 8 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.5wt% of Sn-42-Ag-35-Bi-23 alloy powder (customized by Nangong Dinghong Metal Materials Co., Ltd.) and 0.5wt% of loaded metal single-atom graphene. The metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 42:35:23. The mass ratio of the metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene to the graphene carrier is 1:20.
[0067] A method for preparing a high-strength solder based on SnBi alloy comprises the following steps:
[0068] S1, Preparation of metal-loaded single-atom graphene:
[0069] S1.1 is the same as S1.1 in Example 1, firstly preparing a graphene carrier with surface defect points;
[0070] S1.2, weigh 11.21g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 4.47g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 5.51g of silver nitrate, 9.47g of 1,10-phenanthroline, and 8.16g of glucose into a 1L clean glass beaker, add 800mL of distilled water and 200mL of ethanol into the glass beaker, and ultrasonicate at an ultrasonic frequency of 80kHz and an ultrasonic power of 800W until the metal precursor solution is completely dissolved, and then Then, the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the speed at 500 rpm. The mass ratio of the total mass of the tin single atom, the silver single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:20, that is, 20 g of the graphene carrier with surface-trapped defect sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C and then dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm;
[0071] S1.3, the obtained particle size D 50 =100-200nm solid powder was heated to 220℃ at 4℃ and kept for 20min, then heated to 520℃ at 6℃ / min and kept for 1h, then heated to 750℃ at 6℃ / min and kept for 1h, then cooled to room temperature naturally, and the solid was taken out and ball milled at 100rpm for 60min in a planetary ball mill to obtain a particle size D 50 = 100-200nm metal-loaded single-atom graphene;
[0072] S2, after the precisely measured Sn42Ag35Bi23 alloy powder is melted into liquid state, the precisely measured metal-loaded single-atom graphene prepared in S1.3 is added and stirred for 20 minutes under nitrogen protection, and then cooled and formed to obtain the high-strength solder of SnBi alloy.
[0073] The difference between Example 9 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.5wt% of homemade tin-bismuth alloy powder and 0.5wt% of loaded metal single-atom graphene.
[0074] The homemade tin-bismuth alloy powder is made of the following alloy elements: 43% bismuth Bi, 0.06% tungsten W, 0.5% indium In, 0.12% cobalt Co, 0.15% cerium Ce, and the balance is tin Sn. The eutectic point of the tin-bismuth alloy powder is 140.8°C.
[0075] The metal single atoms loaded on the surface of the graphene carrier in the metal single atom loaded graphene are Sn, Bi, and In. The mass ratio of Sn, Bi, and In loaded on the surface of the graphene carrier is 113:86:1.
[0076] A method for preparing a high-strength solder based on SnBi alloy comprises the following steps:
[0077] S1, Preparation of metal-loaded single-atom graphene:
[0078] S1.1 is the same as S1.1 in Example 1, firstly preparing a graphene carrier with surface defect points;
[0079] S1.2, weigh 15.08g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 8.35g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 0.15g of indium sulfate nonahydrate (CAS No.: 10294-68-5), 9.16g of 1,10-phenanthroline, and 8.54g of glucose into a 1L clean glass beaker, add 800mL of distilled water and 200mL of ethanol to the glass beaker, and ultrasonicate at an ultrasonic frequency of 80kHz and an ultrasonic power of 800W until completely dissolved. The metal precursor solution was obtained, and then the graphene carrier with surface-defective sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the speed at 500 rpm. The mass ratio of the total mass of the tin single atom, the silver single atom and the bismuth single atom to the graphene carrier with surface-defective sites was 1:20, that is, 20 g of the graphene carrier with surface-defective sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain the solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm;
[0080] S1.3, the obtained particle size D 50=100-200nm solid powder was heated to 250℃ at 4℃ and kept for 20min in 4%.v nitrogen-argon mixed gas (nitrogen:argon=94:4), then heated to 580℃ at 6℃ and kept for 1h, then heated to 800℃ at 6℃ / min and kept for 1h, then cooled to room temperature naturally, and the solid was taken out and ball milled in a planetary ball mill at 100rpm for 60min to obtain a particle size D 50 = 100-200nm metal-loaded single-atom graphene;
[0081] S2, according to the formula of homemade tin-bismuth alloy powder: 43% bismuth Bi, 0.06% tungsten W, 0.5% indium In, 0.12% cobalt Co, 0.15% cerium Ce, and the balance is tin. After the accurately measured mixed powder of tin, bismuth, tungsten, indium, cobalt and cerium metals is melted into liquid, the accurately measured loaded metal single atom graphene prepared in S1.3 is added and stirred for 30 minutes under nitrogen protection. After cooling and molding, the high-strength solder of SnBi alloy can be obtained.
[0082] The difference between Example 11 and Example 1 is that the mass ratio of the metal single atom supported on the surface of the graphene carrier in the metal single atom graphene supported is 1:10. The difference in its preparation method is that: S1.2, 11.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 11.26g of bismuth acetylacetonate (Beijing Huoke Technology Co., Ltd. CAS: 141364-06-9) and 10.15g of 1,10-phenanthroline, 8.58g of 2-methylimidazole, 7.24g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency is 80kHz and ultrasonic power is 800W until completely dissolved. The metal precursor solution was obtained, and then the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the speed at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:10, that is, 10 g of the graphene carrier with surface-trapped defect sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0083] The difference between Example 12 and Example 1 is that the mass ratio of the metal single atom supported on the surface of the graphene carrier in the metal single atom graphene to the graphene carrier is 1:25. The difference in its preparation method is as follows: S1.2, 11.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 11.26g of bismuth acetylacetonate (Beijing Huoke Technology Co., Ltd. CAS: 141364-06-9) and 10.15g of 1,10-phenanthroline, 8.58g of 2-methylimidazole, 7.24g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency of 80kHz and ultrasonic power of 800W are used to completely dissolve. The metal precursor solution was obtained, and then the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the speed at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:25, that is, 25 g of the graphene carrier with surface-trapped defect sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0084] The difference between Example 10 and Example 1 is that the mass ratio of the metal single atom supported on the surface of the graphene carrier in the metal single atom graphene to the graphene carrier is 1:50. The difference in its preparation method is that: S1.2, 11.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 11.26g of bismuth acetylacetonate (Beijing Huoke Technology Co., Ltd. CAS: 141364-06-9) and 10.15g of 1,10-phenanthroline, 8.58g of 2-methylimidazole, 7.24g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency is 80kHz and ultrasonic power is 800W until completely The metal precursor solution was dissolved, and then the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:50, that is, 10 g of the graphene carrier with surface-trapped defect sites was added to 20 mL of the metal precursor solution. After the addition was completed, stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50= Solid powder of 100-200nm.
[0085] The difference between Comparative Example 1 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.6wt% of Sn42Bi58 alloy powder and 0.4wt% of graphene (highly conductive graphene TNHRGO from Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences). A method for preparing a high-strength solder based on SnBi alloy is as follows: melt the precisely measured Sn42Bi58 alloy powder to liquid, add graphene (highly conductive graphene TNHRGO from Chengdu Organic Chemistry Co., Ltd., Chinese Academy of Sciences), stir for 15 minutes under nitrogen protection, and cool and shape to obtain a high-strength solder of SnBi alloy.
[0086] The difference between Comparative Example 2 and Example 1 is that the mass ratio of the metal single atom supported on the surface of the graphene carrier in the metal single atom graphene to the graphene carrier is 1:8. The difference in its preparation method is as follows: S1.2, 11.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 11.26g of bismuth acetylacetonate (Beijing Huoke Technology Co., Ltd. CAS: 141364-06-9) and 10.15g of 1,10-phenanthroline, 8.58g of 2-methylimidazole, and 7.24g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency is 80kHz and ultrasonic power is 800W until completely The metal precursor solution was dissolved, and then the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the temperature at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:8, that is, 8 g of the graphene carrier with surface-trapped defect sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0087] The difference between Comparative Example 3 and Example 1 is that the mass ratio of the metal single atom supported on the surface of the graphene carrier in the metal single atom graphene to the graphene carrier is 1:100. The difference in its preparation method is as follows: S1.2, 11.22g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 11.26g of bismuth acetylacetonate (Beijing Huoke Technology Co., Ltd. CAS: 141364-06-9), 10.11g of bismuth acetylacetonate (Beijing Huoke Technology Co., Ltd. CAS: 141364-06-9) and 10.15g of 1,10-phenanthroline, 8.58g of 2-methylimidazole, 7.24g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency is used to heat the glass beaker. The metal precursor solution was completely dissolved by ultrasonic treatment at a rate of 80 kHz and an ultrasonic power of 800 W, and then the graphene carrier with surface-trapped defect sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the temperature at 500 rpm. The mass ratio of the total mass of the tin single atom and the bismuth single atom to the graphene carrier with surface-trapped defect sites was 1:50, that is, 5 g of the graphene carrier with surface-trapped defect sites was added to 20 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0088] The difference between Comparative Example 4 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.97wt% of Sn-42-Bi-58 alloy powder and 0.03wt% of loaded metal single-atom graphene.
[0089] The difference between Comparative Example 5 and Example 1 is that a high-strength solder based on SnBi alloy is made of 97.8wt% of Sn-42-Bi-58 alloy powder and 2.2wt% of loaded metal single-atom graphene.
[0090] The difference between Comparative Example 6 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.6wt% of Sn-42-Bi-58 alloy powder and 0.4wt% of metal-loaded single-atom graphene. The metal single atom loaded on the surface of the graphene carrier in the metal-loaded single-atom graphene is Sn.
[0091] The difference in the preparation method of a high-strength solder based on SnBi alloy is as follows: S1.2, 26.70g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 10.58g of 1,10-phenanthroline, and 8.26g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency of 80kHz and ultrasonic power of 800W are used to completely dissolve the metal precursor solution, and then maintained at 500rp m, add S1.1 graphene carrier with surface trap defect sites into a glass beaker at a rate of 1 g / 20 s, the mass ratio of the total mass of tin single atom, silver single atom and bismuth single atom to the graphene carrier with surface trap defect sites is 1:20, that is, 20 g of graphene carrier with surface trap defect sites is added to 100 mL of metal precursor solution, and the stirring is continued at 500 rpm for 120 min after the addition is completed. After the stirring is completed, the solvent is removed by rotary evaporation at 80 ° C, and then the solid is dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder is wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0092] The difference between Comparative Example 7 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.6wt% Sn-42-Bi-58 alloy powder and 0.4wt% loaded metal single atom graphene. The metal single atom loaded on the surface of the graphene carrier in the loaded metal single atom graphene is Bi.
[0093] The difference in the preparation method of a high-strength solder based on SnBi alloy is that: S1.2, 19.42g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 11.18g of 1,10-phenanthroline, and 7.52g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency of 80kHz and ultrasonic power of 800W are used to completely dissolve the metal precursor solution, and then maintained at 500rpm. The graphene carrier with surface-defective sites of S1.1 was added to a glass beaker at a rate of 1 g / 20 s. The mass ratio of the total mass of tin single atoms, silver single atoms and bismuth single atoms to the graphene carrier with surface-defective sites was 1:20, that is, 20 g of the graphene carrier with surface-defective sites was added to 100 mL of the metal precursor solution. After the addition was completed, stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C and then dried at 80 ° C for 4 h to obtain a solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0094] The difference between Comparative Example 8 and Example 1 is that a high-strength solder based on SnBi alloy is made of 99.6wt% of Sn-42-Bi-58 alloy powder and 0.4wt% of loaded metal single-atom graphene. The metal single atoms loaded on the surface of the graphene carrier in the loaded metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 7:3.
[0095] The difference in the preparation method of a high-strength solder based on SnBi alloy is that: S1.2, 18.68g of bis(acetylacetonate)tin (Shanghai Baishun Biotechnology Co., Ltd., CAS: 16009-86-2), 5.82g of bismuth acetylacetonate (Beijing Hao Ke Technology Co., Ltd. CAS: 141364-06-9), 10.42g of 1,10-phenanthroline, and 8.24g of glucose are added to a 1L clean glass beaker, 800mL of distilled water and 200mL of ethanol are added to the glass beaker, and ultrasonic frequency of 80kHz and ultrasonic power of 800W are used to completely dissolve. The metal precursor solution was obtained, and then the graphene carrier with surface-defective sites of S1.1 was added to the glass beaker at a rate of 1 g / 20 s while maintaining the speed at 500 rpm. The mass ratio of the total mass of the tin single atom, the silver single atom and the bismuth single atom to the graphene carrier with surface-defective sites was 1:20, that is, 20 g of the graphene carrier with surface-defective sites was added to 100 mL of the metal precursor solution. After the addition was completed, the stirring was continued at 500 rpm for 120 min. After the stirring was completed, the solvent was removed by rotary evaporation at 80 ° C, and then the solid was dried at 80 ° C for 4 h to obtain the solid. The obtained solid powder was wet-milled by planetary ball milling to obtain a particle size D 50 = Solid powder of 100-200nm.
[0096] Comparative Example 9 is a Sn42Bi58 alloy solder (Wuxi Fanchuan Tin Industry Co., Ltd.).
[0097] Performance test: Determined according to GBT 2651-2008 welded joint tensile test method.
[0098] Table 1 is a table of test parameters of high strength solder in Examples 1-12 and Comparative Examples 1-9
[0099]
[0100]
[0101] It can be seen from Examples 1-12 and Comparative Examples 1-9 and Table 1 that, compared with Comparative Examples 1 and 9, Example 1 has better compatibility with the metal-loaded single-atom graphene and the tin-bismuth alloy powder in the present application, and can effectively improve the mechanical strength, toughness, thermal conductivity and electrical conductivity of the prepared tin-bismuth alloy solder, which is suitable for the low-temperature packaging requirements of electronic components with special low-temperature packaging requirements such as the most cutting-edge flexible solar panels, thermal sensitive components, solar laminated battery structure devices, etc.
[0102] Combining Examples 1-12 and Comparative Examples 1-9 and Table 1, it can be seen that when Examples 1-5 are compared with Comparative Examples 4-5, the addition amount of loaded metal single-atom graphene is controlled at 0.4-0.8wt%, and the prepared tin-bismuth alloy solder has the best comprehensive performance.
[0103] Combining Examples 1-12 and Comparative Examples 1-9 and Table 1, it can be seen that compared with Comparative Examples 2-3, in Examples 1 and 10-12, the mass ratio of the metal single atom loaded on the surface of the graphene carrier in the metal single atom graphene to the graphene carrier is preferably 1:(10-50), and the preferred range is 1:(20-25), which can ensure that the comprehensive performance of the tin-bismuth alloy solder is better, that is, the compatibility of the metal single atom graphene loaded with metal is better with the tin-bismuth alloy powder.
[0104] Combining Examples 1-12 and Comparative Examples 1-9 and Table 1, it can be seen that compared with Comparative Examples 6-8, Example 1 shows that the metal single atoms loaded on the surface of the graphene carrier in the metal single atom graphene loaded include at least Sn and Bi, and the mass ratio of Sn and Bi is similar to the ratio of alloy elements in the tin-bismuth alloy powder, which can make the compatibility of the metal single atom graphene loaded with the tin-bismuth alloy powder better, thereby ensuring that the prepared tin-bismuth alloy solder has better comprehensive performance.
[0105] Combining Examples 1-12 and Comparative Examples 1-9 and Table 1, it can be seen that compared with Comparative Example 9, Examples 1, 6-9 show that the tin-bismuth alloy solder in Example 6 has the best economic cost, and Examples 7-8 have better comprehensive performance, but the production cost is relatively high, which is suitable for the welding of high-end components. The tin-bismuth alloy solder prepared by combining the homemade tin-bismuth alloy powder in Example 9 with the loaded metal single atom graphene has relatively good comprehensive performance, and the production cost is relatively low compared to the welding in Examples 7-8.
[0106] In summary, the present application uses metal-loaded single-atom graphene to effectively solve the compatibility problem between graphene materials and tin-bismuth alloy powders, compensates for the toughness and brittleness defects of the original tin-bismuth alloy, and gives the prepared tin-bismuth SnBi alloy solder good thermal conductivity, mechanical strength and impact toughness, which can meet the low-temperature packaging requirements of precision electronic devices.
[0107] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A high-strength solder based on SnBi alloy, characterized in that: It is mainly made of tin-bismuth alloy powder and loaded metal single-atom graphene. The content of loaded metal single-atom graphene in the high-strength solder based on SnBi alloy is 0.4-2.0wt%; The metal single atoms loaded on the surface of the graphene carrier in the metal single atom loaded graphene include at least Sn and Bi; The tin-bismuth alloy powder is at least one of tin-42-bismuth-58 alloy powder, tin-57-bismuth-43 alloy powder, tin-52-silver-32-bismuth-16 alloy powder, and tin-42-silver-35-bismuth-23 alloy powder; When the tin-bismuth alloy powder is tin-42-bismuth-58 alloy powder, the metal single atoms supported on the surface of the graphene carrier in the metal single atom-loaded graphene are Sn and Bi, and the mass ratio of Sn to Bi is 42:58; When the tin-bismuth alloy powder is tin-57-bismuth-43 alloy powder, the metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 57:43; When the tin-bismuth alloy powder is a tin-52-silver-32-bismuth-16 alloy powder, the metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 52:32:16; When the tin-bismuth alloy powder is a tin-42-silver-35-bismuth-23 alloy powder, the metal single atoms supported on the surface of the graphene carrier in the metal single-atom graphene are Sn, Ag, and Bi, and the mass ratio of Sn, Ag, and Bi is 42:35:23; Alternatively, the tin-bismuth alloy powder is a homemade tin-bismuth alloy powder, which is made of the following alloy elements: 42-45% bismuth Bi, 0.05-0.2% tungsten W, 0.4-0.8% indium In, 0.05-0.25% cobalt Co, 0.10-0.25% cerium Ce, and the balance is tin Sn; the metal single atoms loaded on the surface of the graphene carrier in the metal single atom graphene are Sn, Bi, and In; the mass ratio of Sn, Bi, and In loaded on the surface of the graphene carrier is 113:86:1; The mass ratio of the metal single atom loaded on the surface of the graphene carrier to the graphene carrier in the metal single atom loaded graphene is 1:(10-50).
2. The high-strength solder based on SnBi alloy according to claim 1, characterized in that: The eutectic point of the Sn-Bi alloy powder is 138-145°C.
3. The high-strength solder based on SnBi alloy according to claim 1, characterized in that: The eutectic point of the Sn42Bi58 alloy powder is 138°C; the eutectic point of the Sn57Bi43 alloy powder is 139°C; the eutectic point of the Sn52Ag32Bi16 alloy powder is 138°C; and the eutectic point of the Sn42Ag35Bi23 alloy powder is 141°C.
4. A high-strength solder based on SnBi alloy according to any one of claims 1 to 3, characterized in that: The tin-bismuth alloy powder is tin-57-bismuth-43 alloy powder, and the eutectic point of the tin-57-bismuth-43 alloy powder is 139° C. The metal single atoms loaded on the surface of the graphene carrier in the metal single-atom graphene are Sn and Bi, and the mass ratio of Sn to Bi is 57:
43.
5. The high-strength solder based on SnBi alloy according to claim 1, characterized in that: The content of the metal-loaded single-atom graphene is 0.4-0.5wt%; the mass ratio of the metal single atom loaded on the surface of the graphene carrier to the graphene carrier in the metal-loaded single-atom graphene is 1:(20-25).
6. The high-strength solder based on SnBi alloy according to claim 1, characterized in that: The number of layers of the graphene carrier in the metal-loaded single-atom graphene is less than 10, the sheet diameter is less than 5 μm, the thickness is less than 5 nm, and the specific surface area is 100-1000 m 2 / g.
7. The high-strength solder based on SnBi alloy according to claim 1, characterized in that: The eutectic point of the tin-bismuth alloy powder is 140-145° C.; the metal single atoms loaded on the surface of the graphene carrier in the metal single atom loaded graphene include at least Sn, Bi, and In.
8. The high-strength solder based on SnBi alloy according to claim 1, characterized in that: The steps are as follows: melt the tin-bismuth alloy powder into a liquid state, add the loaded metal single atom graphene, stir for 10-30 minutes under nitrogen protection, and cool and shape to obtain a high-strength solder based on SnBi alloy.