A nano zinc oxide antibacterial fabric and its production process
Through the surface modification and dispersion technology of nano zinc oxide, the problem of unstable antibacterial performance in textile materials is solved, and the efficient antibacterial effect and good washing resistance of nano zinc oxide textile materials are achieved.
Patent Information
- Application Number
- CN202311784062.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-12-22
AI Technical Summary
The application of nano zinc oxide in textile materials is affected by its surface defects and agglomeration problems, resulting in unstable antibacterial performance and inability to fully exert its excellent biocompatibility and antibacterial activity.
The surface modification of nano zinc oxide is carried out by dispersion technology combined with physical and chemicals. The nano zinc oxide spinning liquid is prepared through hot melting, radiation crosslinking and laser precipitation. Combined with ultrasonic oscillation and spinning technology, it ensures uniform nano zinc oxide. Dispersed in the fibers, forming a stable structure to improve antibacterial effect.
It significantly improves the photostability and antibacterial properties of nano zinc oxide, enhances the water resistance and antibacterial properties of the fiber, ensures effective bactericidal effect on bacteria, and maintains good antibacterial properties after multiple washings.
Smart Images

Figure BDA0004624605240000061 
Figure BDA0004624605240000062 
Figure BDA0004624605240000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile materials, and in particular to a nano zinc oxide antibacterial fabric and a production process. Background Art
[0002] Nano zinc oxide composite textile fabric refers to the nano zinc oxide coated or wrapped inside the fiber by physical and chemical means. Since nano zinc oxide particles have the unique surface effect of nano materials, strong catalytic efficiency, macro quantum tunneling effect and small size effect, they have special properties that ordinary zinc oxide does not have in terms of magnetism, electricity, light, heat, etc. At the same time, nano zinc oxide has excellent physical and chemical properties in ultraviolet shielding, magnetic materials, and anti-shade disinfection, and has broad development prospects. Nano zinc oxide is a new type of multifunctional inorganic nanomaterial. Due to its large specific surface area and high surface energy, nano zinc oxide is very easy to agglomerate in liquid media and cannot be evenly dispersed in the spinning solution, which not only affects the smooth spinning, but also makes it difficult to give full play to the various excellent properties of nano zinc oxide. Compared with other antibacterial materials, as a traditional wide bandgap semiconductor, zinc oxide has excellent biocompatibility, antibacterial activity, good thermal stability and long-term effectiveness. It is used in various biomedical fields and is a promising antibacterial agent. The interaction between zinc oxide particles and bacteria is more effective when their size is reduced to the nanoscale, and most bacteria are lethal. Nano zinc oxide exhibits excellent antibacterial activity against a broad spectrum of bacteria, but when nano zinc oxide is used alone, reactive oxygen species can be generated on its surface, and the e- and h+ generated by light excitation will recombine, thereby reducing the generation of reactive oxygen species and reducing antimicrobial activity;
[0003] As people's living standards improve, textile fabrics need to have anti-fouling and anti-bacterial functions to a certain extent. At present, there are two main ways to use anti-bacterial fabrics. One is to use the anti-bacterial, moisture-absorbing and health-care functions of natural fibers themselves, and the other is to use processing technology to add or impregnate particles or ions with anti-bacterial functions into the fabric. Although the former has higher environmental health, its anti-bacterial performance is often insufficient and cannot meet the anti-bacterial requirements of the fabric. When the latter is treated with anti-fouling and anti-bacterial treatment, due to different methods of external introduction, its anti-bacterial effect is not good, and the stability is poor. After repeated washing, the anti-bacterial effect will be greatly weakened. Summary of the invention
[0004] In view of this, the present invention proposes a nano zinc oxide antibacterial fabric and a production process to solve the above problems.
[0005] The technical solution of the present invention is achieved as follows: a nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 80-100 parts of spinning solution, 15-33 parts of nano zinc oxide, 2-5 parts of cross-linking agent, and 2-8 parts of dispersion solution; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of (5-8):(1-3):(0.2-1.1).
[0006] Furthermore, a nano zinc oxide antibacterial fabric includes the following raw materials in parts by weight: 90 parts of spinning solution, 28 parts of nano zinc oxide, 3 parts of cross-linking agent, and 5 parts of dispersion liquid.
[0007] Furthermore, the cross-linking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of (2.5-5.9):(8.8-12.7):(0.3-1.2).
[0008] Furthermore, the dispersion is selected from sodium dodecylbenzenesulfonate, hexadecyltrimethylammonium bromide, and polyethylene glycol.
[0009] Furthermore, a production process of nano zinc oxide antibacterial fabric comprises the following steps:
[0010] Step S1, preparing spinning solution: heat-melting polyacrylonitrile, adding the above-mentioned mint fiber and tea fiber, mixing and stirring for 50-120 minutes to obtain a hot melt solution, immersing in a 30-50wt% sodium thiocyanate solution at a temperature of 80-120°C, and simultaneously performing radiation cross-linking for 1-3 hours, the power of the radiation source is 13-20W, the radiation dose is 0.04-0.7kGy, degassing treatment is performed for 3-6 hours at a temperature of 76-92°C and a vacuum degree of 0.1-0.6MPa to obtain a spinning solution for standby use;
[0011] Step S2, preparing a nano zinc oxide suspension: immersing the nano zinc oxide in a crosslinking agent, stirring and mixing at a temperature of 50-80° C., filling with nitrogen, and placing in a laser generator for laser precipitation to obtain a nano zinc oxide suspension for standby use;
[0012] Step S3, dispersion: mixing the nano zinc oxide suspension and dispersion into the spinning solution, and simultaneously subjecting the mixture to ultrasonic oscillation treatment for 3-8 hours to obtain the nano zinc oxide spinning solution;
[0013] Step S4, spinning and weaving: the zinc oxide spinning solution prepared in S3 is extruded through a spinneret, and then sprayed out through the spinneret and passed through -3 to -1°C cooling water to obtain frozen collagen filaments, which are then woven to obtain nano zinc oxide antibacterial fabrics.
[0014] Compared with the prior art, the present invention has the following beneficial effects:
[0015] The present invention adopts physical and chemical combined dispersion to modify the surface of nano zinc oxide, thereby reducing its surface defects, inhibiting the composite effect of negative charges and hydrogen ions, and improving the separation efficiency of nano zinc oxide photogenerated electron-hole pairs. + ) undergoes oxidation reaction, negative charges and hydrogen ions react with oxygen and water on the surface of nano zinc oxide particles to generate chemically active active oxygen, which can cut the chemical bonds of bacterial organic matter to achieve a bactericidal effect, and also improves light stability and enhances photocatalytic activity;
[0016] The raw materials of the spinning solution are selected according to a suitable formula. The molecular structure of the cellulose in the spinning solution obtained by heat melting and radiation cross-linking contains a large number of hydroxyl groups, which makes the cellulose highly hydrophilic and can form hydrogen bonds with water molecules, thereby increasing the water resistance and antibacterial properties of the fiber;
[0017] The surface-modified nano zinc oxide is dispersed in the spinning solution, and can penetrate the nano zinc oxide into the spinning solution to form a stable structure that is not easy to agglomerate. It can be evenly loaded on the fiber to achieve full contact with bacteria, thereby obtaining better antibacterial effect and good washing resistance. DETAILED DESCRIPTION
[0018] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.
[0019] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.
[0020] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.
[0021] Example 1
[0022] A nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 80 parts of spinning solution, 15 parts of nano zinc oxide, 2 parts of crosslinking agent, and 2 parts of dispersion liquid; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of 5:1:0.2; the crosslinking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of 2.5:8.8:0.3; and the dispersion liquid is selected from sodium dodecylbenzene sulfonate.
[0023] Example 2
[0024] A nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 100 parts of spinning solution, 33 parts of nano zinc oxide, 5 parts of crosslinking agent, and 8 parts of dispersion liquid; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of 8:3:1.1; the crosslinking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of 5.9:12.7:1.2; and the dispersion liquid is selected from hexadecyltrimethylammonium bromide.
[0025] Example 3
[0026] A nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 90 parts of spinning solution, 28 parts of nano zinc oxide, 3 parts of crosslinking agent, and 5 parts of dispersion liquid; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of 7:2:0.8; the crosslinking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of 4.1:10.2:0.9; the dispersion liquid is selected from polyethylene glycol;
[0027] The above-mentioned embodiments 1-3 adopt the following production process:
[0028] Step S1, preparing spinning solution: heat-melting polyacrylonitrile, adding the above-mentioned mint fiber and tea fiber, mixing and stirring for 80 minutes to obtain a hot melt solution, immersing in a 40wt% sodium thiocyanate solution at a temperature of 100°C, and simultaneously performing radiation cross-linking for 2 hours, the power of the radiation source is 17W, the radiation dose is 0.4kGy, degassing treatment is performed for 4 hours at a temperature of 80°C and a vacuum degree of 0.4MPa to obtain a spinning solution for standby use;
[0029] Step S2, preparing a nano zinc oxide suspension: immersing the nano zinc oxide in a crosslinking agent, stirring and mixing at a temperature of 70° C., filling with nitrogen, and placing in a laser generator for laser precipitation to obtain a nano zinc oxide suspension for standby use;
[0030] Step S3, dispersion: mixing the nano zinc oxide suspension and dispersion into the spinning solution, and simultaneously subjecting the mixture to ultrasonic oscillation treatment for 5 hours to obtain the nano zinc oxide spinning solution;
[0031] Step S4, spinning and weaving: the zinc oxide spinning solution prepared in S3 is extruded through a spinneret, then sprayed out through the spinneret and passed through -2°C cooling water to obtain frozen collagen filaments, which are then woven to obtain nano zinc oxide antibacterial fabrics.
[0032] Example 4
[0033] A nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 90 parts of spinning solution, 28 parts of nano zinc oxide, 3 parts of crosslinking agent, and 5 parts of dispersion liquid; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of 7:2:0.8; the crosslinking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of 4.1:10.2:0.9; the dispersion liquid is selected from polyethylene glycol;
[0034] The above embodiment adopts the following production process:
[0035] Step S1, preparing spinning solution: heat-melting polyacrylonitrile, adding the above-mentioned mint fiber and tea fiber, mixing and stirring for 50 minutes to obtain a hot melt solution, immersing in a 30wt% sodium thiocyanate solution at a temperature of 80°C, and simultaneously performing radiation cross-linking for 1 hour, the power of the radiation source is 13W, the radiation dose is 0.04kGy, degassing treatment is performed at a temperature of 76°C and a vacuum degree of 0.1MPa for 3 hours to obtain a spinning solution for standby use;
[0036] Step S2, preparing a nano zinc oxide suspension: immersing the nano zinc oxide in a crosslinking agent, stirring and mixing at a temperature of 50° C., filling with nitrogen, and placing in a laser generator for laser precipitation to obtain a nano zinc oxide suspension for standby use;
[0037] Step S3, dispersion: mixing the nano zinc oxide suspension and dispersion into the spinning solution, and simultaneously subjecting the mixture to ultrasonic oscillation for 3 hours to obtain the nano zinc oxide spinning solution;
[0038] Step S4, spinning and weaving: the zinc oxide spinning solution prepared in S3 is extruded through a spinneret, and then sprayed out through the spinneret and passed through -3°C cooling water to obtain frozen collagen filaments, which are then woven to obtain nano zinc oxide antibacterial fabrics.
[0039] Example 5
[0040] A nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 90 parts of spinning solution, 28 parts of nano zinc oxide, 3 parts of crosslinking agent, and 5 parts of dispersion liquid; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of 7:2:0.8; the crosslinking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of 4.1:10.2:0.9; the dispersion liquid is selected from polyethylene glycol;
[0041] The above embodiment adopts the following production process:
[0042] Step S1, preparing spinning solution: heat-melting polyacrylonitrile, adding the above-mentioned mint fiber and tea fiber, mixing and stirring for 12 minutes to obtain a hot melt solution, immersing in a 50wt% sodium thiocyanate solution at a temperature of 120°C, and simultaneously performing radiation cross-linking for 3 hours, the power of the radiation source is 20W, the radiation dose is 0.7kGy, degassing treatment is performed at a temperature of 92°C and a vacuum degree of 0.6MPa for 6 hours to obtain a spinning solution for standby use;
[0043] Step S2, preparing a nano zinc oxide suspension: immersing the nano zinc oxide in a crosslinking agent, stirring and mixing at a temperature of 80° C., filling with nitrogen, and placing in a laser generator for laser precipitation to obtain a nano zinc oxide suspension for standby use;
[0044] Step S3, dispersion: mixing the nano zinc oxide suspension and dispersion into the spinning solution, and simultaneously subjecting the mixture to ultrasonic oscillation treatment for 8 hours to obtain the nano zinc oxide spinning solution;
[0045] Step S4, spinning and weaving: the zinc oxide spinning solution prepared in S3 is extruded through a spinneret, then sprayed out through the spinneret and passed through -1°C cooling water to obtain frozen collagen filaments, which are then woven to obtain nano zinc oxide antibacterial fabrics.
[0046] Comparative Example 1
[0047] The difference between this comparative example and Example 3 is that a nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 70 parts of spinning solution, 10 parts of nano zinc oxide, 8 parts of cross-linking agent, and 1 part of dispersion.
[0048] Comparative Example 2
[0049] The difference between this comparative example and Example 3 is that the nano zinc oxide in the nano zinc oxide antibacterial fabric is not immersed in the cross-linking agent.
[0050] Comparative Example 3
[0051] The difference between this comparative example and Example 3 is that the spinning solution does not contain mint fiber and tea fiber.
[0052] 1. Antibacterial Test
[0053] The antibacterial fabrics prepared in Examples 1-5 of the present invention and Comparative Examples 1-3 were subjected to the antibacterial test method specified in GB / T20944.3-2008 "Evaluation of Antibacterial Properties of Textiles Part 3: Oscillation Method", and the antibacterial properties of the antibacterial fabrics of the present invention against Escherichia coli, Staphylococcus aureus, and Candida albicans were measured by plate counting method to determine the proliferation of bacterial colonies;
[0054] The inhibition rate was calculated according to the following formula:
[0055]
[0056] Where A is the number of colonies in the centrifuge tube after the antibacterial fabric was oscillated at constant temperature for 24 hours, and B is the number of colonies in the centrifuge tube of the blank control sample.
[0057] The test results are shown in Table 1:
[0058]
[0059]
[0060] The above results show that the antibacterial fabric of the present invention has good antibacterial performance. After 20 washes, it shows good antibacterial performance. In particular, the antibacterial fabric prepared in the step of Example 3 has an antibacterial performance of 98.9% against Escherichia coli, 99.9% against Staphylococcus aureus, and 97.8% against Candida albicans. This shows that after nano zinc oxide is immersed in the cross-linking agent as a metal oxide, ROS is generated and the released Zn 2+ Ions may penetrate the bacterial cell membrane, bind to intracellular proteases, poison the enzymes, disrupt intracellular metabolism, and inhibit bacterial growth.
[0061] 2. Washable and antibacterial performance test
[0062] Referring to the simplified washing process and operating conditions of Appendix C of FZ / T73023-2006 "Antibacterial Knitwear", the antibacterial fibers of Example 3 and Comparative Examples 2 and 3 of the present invention were washed. A standard detergent solution with a concentration of 2 g / L was prepared as a washing liquid. According to a bath ratio of 1:30 between the sample and the washing liquid, the bottle was placed in a constant temperature water bath oscillator (oscillation frequency 150 rpm, water temperature 40°C, time 5 min) for oscillation washing. After washing, the sample was taken out and washed several times with deionized water until there was no residual washing liquid on the fiber. This was repeated 20 times, 30 times and 50 times as one washing process. Three parallel samples were made for each sample. The bacterial proliferation was determined by the plate count method. The antibacterial rate was calculated according to the above formula. The determination results are as follows:
[0063] Table 2:
[0064]
[0065] Table 3:
[0066]
[0067]
[0068] Table 4:
[0069]
[0070] From the results of its water-washing antibacterial property in Tables 2-4, it can be seen that the antibacterial fabric of Example 3 does not show a significant downward trend with the increase in the number of washing times. After washing 20 times, the antibacterial property of Escherichia coli is 98.6%, the antibacterial property of Staphylococcus aureus is 99.5%, and the antibacterial property of Candida albicans is 97.5%. After washing 30 times, the antibacterial property of Escherichia coli is 98.1%, the antibacterial property of Staphylococcus aureus is 99.3%, and the antibacterial property of Candida albicans is 95.8%. After washing 50 times, the antibacterial property of Escherichia coli is 98.4%, the antibacterial property of Staphylococcus aureus is 99.4%, and the antibacterial property of Candida albicans is 97.2%.
[0071] After washing, the antibacterial performance of Comparative Example 2 was significantly reduced. It can be seen that the cross-linking agent cross-linked the functional groups on the surface of the nano zinc oxide particles to form a cross-linked network structure, which can improve its light resistance, water resistance and solvent resistance.
[0072] Comparative Example 3 illustrates that the textile structure adding mint fiber and tea fiber surface can limit the adsorption and colonization of bacteria, and prevent the formation of colonies, and the micro-space between fibers can limit the diffusion of bacteria, thereby inhibiting the growth of bacteria on the fiber, and at the same time, mint fiber and tea fiber contain natural antibacterial substances, which can inhibit the growth and reproduction of bacteria through penetration or release mechanism. When the fiber is in contact with water or other liquids, the antibacterial substances will be gradually released to form a kind of antibacterial effect. In addition, the molecular structure of cellulose in the obtained spinning solution contains a large amount of hydroxyl groups, so that cellulose has a higher hydrophilicity, can form hydrogen bonds with water molecules, thereby increasing the water resistance of the fiber.
[0073] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A production process of nano zinc oxide antibacterial fabric, characterized in that: The following steps are involved: Step S1, preparing spinning solution: heat-melting polyacrylonitrile, adding mint fiber and tea fiber, mixing and stirring for 50-120 minutes to obtain a hot melt solution, immersing in a 30-50wt% sodium thiocyanate solution at a temperature of 80-120° C., and simultaneously performing radiation cross-linking for 1-3 hours, the power of the radiation source is 13-20W, the radiation dose is 0.04-0.7 kGy, and degassing treatment is performed for 3-6 hours at a temperature of 76-92° C. and a vacuum degree of 0.1-0.6 MPa to obtain a spinning solution for standby use; Step S2, preparing a nano zinc oxide suspension: immersing the nano zinc oxide in a crosslinking agent, stirring and mixing at a temperature of 50-80° C., filling with nitrogen, and placing in a laser generator for laser precipitation to obtain a nano zinc oxide suspension for standby use; Step S3, dispersion: mixing the nano zinc oxide suspension and the dispersant into the spinning solution, and simultaneously subjecting the mixture to ultrasonic oscillation treatment for 3-8 hours to obtain the nano zinc oxide spinning solution; Step S4, spinning and weaving: the nano zinc oxide spinning solution prepared in S3 is extruded through a spinneret, and then sprayed out through the spinneret and passed through -3~-1°C cooling water to obtain frozen collagen yarn, which is then spun and processed to obtain nano zinc oxide antibacterial fabric; The thermal melting temperature of step S1 is 230-270°C; The nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 80-100 parts of spinning solution, 15-33 parts of nano zinc oxide, 2-5 parts of crosslinking agent, and 2-8 parts of dispersant; the spinning solution is prepared by mixing polyacrylonitrile, mint fiber, and tea fiber in a mass ratio of (5-8):(1-3):(0.2-1.1); the crosslinking agent is stearic acid, N,N-methylenebisacrylamide, and hydroxyethyl acrylate in a mass ratio of (2.5-5.9):(8.8-12.7):(0.3-1.2); The dispersant is selected from sodium dodecylbenzene sulfonate, hexadecyltrimethylammonium bromide, and polyethylene glycol.
2. The production process of a nano zinc oxide antibacterial fabric as claimed in claim 1, characterized in that: The nano zinc oxide antibacterial fabric comprises the following raw materials in parts by weight: 90 parts of spinning solution, 28 parts of nano zinc oxide, 3 parts of crosslinking agent and 5 parts of dispersant.
3. The production process of a nano zinc oxide antibacterial fabric as claimed in claim 1, characterized in that: The radiation cross-linking in step S1 uses β rays, neutron rays or γ rays.
4. The production process of a nano zinc oxide antibacterial fabric as claimed in claim 1, characterized in that: The laser generator in step S2 has an average laser power of 1.2-2.5 kW, a wavelength of 1010-1080 nm, a repetition frequency of 28-35 MHz, and a pulse width of 100-300 fs.
5. The production process of a nano zinc oxide antibacterial fabric as claimed in claim 1, characterized in that: In step S3, the ultrasonic frequency is 20-40kHz, the power is 10-30W, and the current is 0.1-2.0A.
6. The production process of a nano zinc oxide antibacterial fabric as claimed in claim 1, characterized in that: The spinning conditions of step S4 are: relative humidity 40-60%, temperature 22-28° C., voltage 10-20 kV, and flow rate of spinning solution 0.5-1.5 mL / h.
7. A nano zinc oxide antibacterial fabric made by the production process of the nano zinc oxide antibacterial fabric according to any one of claims 1 to 6.