Biaxially oriented polypropylene electrical film and preparation method thereof
By adding nuclear titanium dioxide to the BOPP electrical film formula and adjusting the production process, the problems of insufficient breakdown strength, resistivity and temperature resistance of the electrical film are solved, achieving higher charge capacity and service life, while simplifying production process and reduce costs.
Patent Information
- Application Number
- CN202311855925.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-29
AI Technical Summary
Existing biaxially oriented polypropylene (BOPP) electrical films suffer from static electricity and adhesion between films during the production process, and their breakdown strength, resistivity and temperature resistance are insufficient, resulting in capacitors being easily damaged during use and production The process is complex and costly.
By adding nuclear titanium dioxide to the formula of the BOPP electrical film, and thoroughly mixing it during high-speed stirring and extrusion, a prefabricated masterbatch A was prepared. The electrical film was prepared by adjusting the original BOPP production line, and its breakdown strength, Resistivity and heat shrink properties.
It effectively improves the breakdown strength, resistivity and temperature resistance of BOPP electrical film, reduces thermal shrinkage, increases the charge capacity and service life of film capacitors, while simplifying the production process and reducing costs.
Smart Images

Figure CN117866255B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of film capacitors, in particular to a biaxially oriented polypropylene electrical film and a preparation method thereof. Background Art
[0002] Film capacitors are widely used in electronics, home appliances, communications, electricity and other fields. With the rapid development of industries such as national power grid construction, high-speed rail construction and new energy electric vehicle manufacturing, the application field of film capacitors is also expanding rapidly. Biaxially oriented polypropylene (BOPP) electrical film is the main dielectric material of film capacitors, accounting for about 70% of the production cost of film capacitors. The quality of electrical film directly affects the performance indicators of capacitors such as stable capacity, excellent voltage resistance, insulation resistance performance, safety of use and life cycle. The acquisition rate of finished products produced by electrical film is low, the quality control requirements are high, and the process technology is very difficult. It is a high value-added product.
[0003] Most of the existing biaxially oriented polypropylene (BOPP) electrical films have the following disadvantages:
[0004] The production process of BOPP electrical film requires a series of processes such as extrusion, stretching, conveying, and surface treatment (corona treatment). Static electricity and sticking between films will occur on the surface of the film. In order to avoid sticking between films, a special process is required to roughen the surface of the film.
[0005] BOPP electrical film requires that the raw materials must not contain additives such as antistatic agents and lubricants. The introduction of any additives will cause the breakdown strength of BOPP electrical film to decrease. Therefore, the production formula is very simple, with only one raw material, polypropylene (PP) resin. In order to roughen the surface of the film, the work of film manufacturers mainly focuses on selecting suitable PP raw materials or achieving it through special production processes. This brings certain complexity to the production process. Therefore, the production of BOPP electrical film requires special biaxial stretching equipment or equipment modification of conventional BOPP film production lines, which is very expensive.
[0006] During the use of capacitors, as the charge storage increases, the temperature of the capacitor gradually rises, and there is a risk of charge breakdown of the film, which in turn causes damage to the capacitor. Therefore, in order to avoid the above situation, there are three main directions for improving the performance of BOPP electrical film: first, improving the breakdown strength of BOPP electrical film, second, improving the resistivity of BOPP electrical film, and third, improving the temperature resistance of BOPP electrical film. For the first two performance improvement directions (breakdown strength, resistivity), film manufacturers mainly achieve this by selecting suitable PP raw materials; and the improvement of temperature resistance can also be adjusted by certain processes on the premise of determining the PP raw materials.
[0007] In summary, it is of great significance to develop a biaxially oriented polypropylene electrical film with high breakdown strength, resistivity and temperature resistance. Summary of the invention
[0008] The object of the present invention is to provide a biaxially oriented polypropylene electrical film and a preparation method thereof, so as to solve the problems in the above-mentioned background technology.
[0009] To achieve the above object, the present invention provides the following technical solution: In a first aspect, the present invention provides a method for preparing a biaxially oriented polypropylene electrical film, comprising the following steps:
[0010] S1, according to the formula, weigh a certain amount of pure PP, nuclear titanium dioxide, and dispersant;
[0011] S2, putting the weighed raw materials into a high-speed stirrer and starting stirring to fully mix them;
[0012] S3, start the granulator and extrude;
[0013] S4, sucking the uniformly mixed raw materials into an extruder, and preparing a prefabricated masterbatch A through extrusion-cooling-pelletizing;
[0014] S5, setting the blanking ratio of PP and prefabricated masterbatch A in the blanking area of the BOPP production line according to a certain ratio;
[0015] S6, other BOPP production parameters remain unchanged, and BOPP electrical film is prepared;
[0016] S7, S7, focus on testing breakdown strength, volume resistivity, thermal shrinkage and surface roughness, and compare with BOPP electrical film made of pure PP.
[0017] Preferably, the contents of the components in the formula in parts by weight are as follows:
[0018] 80-90 parts of pure PP, 10-20 parts of nuclear titanium dioxide, and 0-2 parts of dispersant.
[0019] Preferably, the dispersant in S1 is one or more of a titanate coupling agent, an aluminate coupling agent, an aluminozirconate coupling agent, a silane coupling agent, and stearic acid.
[0020] Preferably, the stirring time in S2 is 5 to 15 minutes.
[0021] Preferably, the extrusion temperature in S3 is 160-220°C.
[0022] Preferably, the conditions for testing the breakdown strength in S7 are a temperature of 85° C. and a relative humidity of 85%.
[0023] The second aspect of the present invention provides a biaxially oriented polypropylene electrical film, wherein the biaxially oriented polypropylene electrical film is prepared by the method described in the first aspect of the present invention.
[0024] The present invention has at least the following beneficial effects:
[0025] (1) The present invention provides a biaxially oriented polypropylene electrical film and a preparation method thereof. Adding nuclear titanium dioxide to the formula can effectively reduce the generation of space charge, reduce the frequency of carrier trapping and detrapping, scatter carriers, weaken the carrier energy, and thus effectively improve the breakdown strength of the polypropylene electrical film;
[0026] (2) The present invention provides a biaxially oriented polypropylene electrical film and a preparation method thereof, which can improve the resistivity and thus improve the charge capacity of the film capacitor;
[0027] (3) The present invention provides a biaxially oriented polypropylene electrical film and a preparation method thereof, which reduces thermal shrinkage, thereby facilitating the improvement of the temperature resistance of the film capacitor during use;
[0028] (4) The present invention provides a biaxially oriented polypropylene electrical film and a preparation method thereof, wherein nuclear titanium dioxide is added to the formula, and the nuclear titanium dioxide particles are dispersed in and outside the film, thereby improving the roughness of the BOPP electrical film. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the surface structure of the biaxially oriented polypropylene electrical film of the present invention. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The present invention provides a method for preparing a biaxially oriented polypropylene electrical film, comprising the following steps:
[0032] S1, according to the formula, weigh a certain amount of pure PP (80-90 parts), nuclear titanium dioxide (10-20 parts), and dispersant (0-2 parts, one or a combination of titanate coupling agent, aluminate coupling agent, aluminozirconate coupling agent, silane coupling agent, and stearic acid);
[0033] S2, putting the weighed raw materials into a high-speed stirrer, stirring for 5 to 15 minutes to fully mix them;
[0034] S3, start the granulator, extrusion temperature 160 ~ 220 ° C;
[0035] S4, sucking the uniformly mixed raw materials into an extruder, and preparing a prefabricated masterbatch A through extrusion-cooling-pelletizing;
[0036] S5, set the blanking ratio of the blanking area of the BOPP production line according to a certain ratio, pure PP (100 parts), prefabricated masterbatch A (final nuclear titanium dioxide addition amount 0.1 to 3 parts);
[0037] S6, other BOPP production parameters remain unchanged, and BOPP electrical film is prepared;
[0038] S7, focusing on testing the breakdown strength (temperature 85°C, relative humidity 85%), volume resistivity, thermal shrinkage and surface roughness, and comparing with BOPP electrical film made of pure PP.
[0039] Based on the above technical solution, the present invention provides the following embodiments and comparative examples, as shown in the following table:
[0040]
[0041]
[0042] Figure 1 It is a schematic diagram of the surface structure of the biaxially oriented polypropylene electrical film of the present invention.
[0043] The present invention has the following advantages:
[0044] 1. Under the same process, the roughness of BOPP electrical film is improved only by adjusting the formula, and the means of adjusting the roughness are expanded. The original preparation method can only be implemented by PP selection and process implementation:
[0045] This is caused by two reasons: First, the nuclear titanium dioxide particles are dispersed in the film, playing the role of heterogeneous nucleating agent, introducing crystal nuclei into PP molecules, and improving the ability of PP molecules to form β crystals. β crystals are unstable and will transform into α crystals at a certain temperature. The sizes of the two crystal forms are different, which leads to the uneven surface of the film; in addition, inevitably, some of the nuclear titanium dioxide particles will be dispersed on the surface of the PP film, and some will be exposed outside the film, which also increases the surface roughness of the PP film. Figure 1 .
[0046] 2. Adding nuclear titanium dioxide to the formula does not reduce the breakdown strength of BOPP electrical film, but is beneficial to improve the breakdown strength:
[0047] In the production of BOPP electrical film, if any additives can be introduced, the additives will cause charge enrichment, thereby greatly reducing the breakdown strength of the film.
[0048] Nuclear titanium dioxide has the advantages of good compatibility with polypropylene, good dispersibility, small and uniform particle size, large specific surface area, and small addition amount. It can effectively reduce the generation of space charge, reduce the frequency of carrier trapping and detrapping, scatter carriers, and weaken carrier energy, thereby effectively improving the breakdown strength of polypropylene electrical film.
[0049] 3. The increase in volume resistivity is beneficial to improving the charge capacity of film capacitors:
[0050] In the film, as the number of core titanium dioxide in the system increases, the transfer of charges is hindered and the transfer capacity is weakened, resulting in an increase in volume resistivity.
[0051] 4. The reduction of thermal shrinkage is conducive to improving the temperature resistance of film capacitors during use:
[0052] In the embodiment system, the PP molecular chain is wrapped around the core titanium dioxide particles, which anchors the PP molecular chain and hinders the relative movement of the PP molecular chain, thereby reducing the mobility of the PP molecular chain during heating and ultimately reducing the thermal shrinkage of the film.
[0053] The above shows and describes the basic principles, main features and advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a biaxially oriented polypropylene electrical film, It is characterized in that The following steps are involved: S1, according to the formula, weigh a certain amount of pure PP, nuclear titanium dioxide, and dispersant; S2, putting the weighed raw materials into a high-speed stirrer and starting stirring to fully mix them; S3, start the granulator and extrude; S4, sucking the uniformly mixed raw materials into an extruder, and preparing a prefabricated masterbatch A through extrusion-cooling-pelletizing; S5, setting the blanking ratio of PP and prefabricated masterbatch A in the blanking area of the BOPP production line according to a certain ratio; S6, other BOPP production parameters remain unchanged, and BOPP electrical film is prepared; S7, focusing on testing breakdown strength, volume resistivity, thermal shrinkage and surface roughness, and comparing with BOPP electrical film made of pure PP; The contents of the components in the formula S1 are as follows in parts by weight: Pure PP 80-90 parts, nuclear titanium dioxide 10-20 parts, dispersant 0-2 parts; The dispersant in S1 is one or more of a titanate coupling agent, an aluminate coupling agent, an aluminozirconate coupling agent, a silane coupling agent, and stearic acid.
2. The method for preparing a biaxially oriented polypropylene electrical film according to claim 1, It is characterized in that The stirring time in S2 is 5 to 15 minutes.
3. The method for preparing a biaxially oriented polypropylene electrical film according to claim 1, It is characterized in that The extrusion temperature in S3 is 160-220°C.
4. The method for preparing a biaxially oriented polypropylene electrical film according to claim 1, It is characterized in that The conditions for testing the breakdown strength in S7 are a temperature of 85° C. and a relative humidity of 85%.
5. A biaxially oriented polypropylene electrical film, It is characterized in that The biaxially oriented polypropylene electrical film is prepared by the method according to any one of claims 1 to 4.