A combined recycling method for ternary materials
Through microwave-assisted hydrogen reduction method and phosphorus-modified graphene purification technology, the separation problem of lithium, nickel, cobalt and manganese in lithium battery recycling is solved, and efficient and environmentally friendly ternary material recycling is achieved, which improves the recovery rate of lithium and Product purity simplifies process flow and reduces energy consumption and pollution.
Patent Information
- Application Number
- CN202311731431.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-12-15
AI Technical Summary
The existing lithium battery recycling methods have problems such as high energy consumption, toxic gas generation, cumbersome operation, difficulty in controlling and secondary pollution, and it is difficult to effectively recover lithium, nickel, cobalt and manganese in ternary materials.
The ternary positive electrode waste was ground by microwave-assisted hydrogen reduction method and microwave-reduced at 550°C to 700°C. Then, react with water and magnetically sorted to separate nickel, cobalt and manganese. The leaching phase was purified by phosphorus modified graphene. Finally, High purity lithium carbonate was obtained by carbonate precipitation.
It realizes efficient selective reduction and separation of lithium, nickel, cobalt and manganese, reduces the impurity ion content in the leaching liquid, improves the recovery rate of lithium and product purity, simplifies the process flow, and reduces energy consumption and pollution emissions.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a combined recovery method of ternary materials. Background Art
[0002] Lithium-ion batteries have the advantages of long cycle life, high specific energy, small self-discharge effect, small size, high operating voltage, no memory effect, wide applicable temperature range, and green environmental protection. They are widely used in 3C products, automobiles, electric vehicles and other fields. With the continuous innovation of lithium-ion battery technology, a variety of batteries have been developed, such as: LiCoO2, LiMn2O4, LiNiO2, LiFePO4 and LiNi x Co y Mn z O2 (x + y + z = 1) battery, etc., in which LiNi x Co y Mn z O2 has attracted widespread attention due to its good thermal stability, high energy density and low production cost.
[0003] The general lifespan of lithium batteries is 3 to 5 years. It can be foreseen that the number of waste ternary lithium batteries will increase significantly. Therefore, it is urgently necessary to develop relevant technical methods to recycle them in order to cope with their impact on the environment and waste of resources.
[0004] At present, the recycling methods of waste ternary lithium batteries are mainly divided into pyrometallurgy, hydrometallurgy and biometallurgy. Pyrometallurgy has strong adaptability to raw materials and rapid reaction, which is suitable for industrial batch processing, but it consumes a lot of energy (melting temperature>1500℃) and produces toxic gases. The bacteria required for biometallurgy have high environmental requirements and a long metal extraction cycle, which makes it difficult to apply in industry. Hydrometallurgy has been widely studied due to its advantages such as mild conditions, low energy consumption and high selectivity for metals, such as organic or inorganic reduction acid leaching and reduction ammonium leaching, but it has defects such as long process flow, cumbersome operation, difficult control, large consumption of acid and alkali reagents, large discharge of three wastes, and easy to cause secondary pollution. Summary of the invention
[0005] The object of the present invention is to provide a combined recovery method of ternary materials to solve at least one aspect of the problems and defects raised in the above-mentioned background technology.
[0006] Specifically, the present invention provides a combined recovery method of ternary materials, comprising:
[0007] S1. Grind the ternary cathode waste into powder, introduce hydrogen into the powder and mix evenly, then perform microwave reduction at 550°C to 700°C to obtain a reduced product;
[0008] The power of the microwave is 1 kW to 3 kW, and the frequency of the microwave is 1 GHZ to 1.5 GHZ;
[0009] S2, placing the reduced product into water for full reaction, and then filtering to obtain leaching residue and leaching phase;
[0010] Magnetic separation of nickel and / or cobalt and / or manganese from the leached residue for subsequent recovery;
[0011] S3, purifying the leached phase and the phosphorus-modified graphene after mixing to obtain a purified solution;
[0012] The method for preparing the phosphorus-modified graphene comprises the following steps:
[0013] The graphene oxide, phosphoric acid solution, polyethylene glycol and water are mixed and then hydrothermally treated to obtain phosphorus-modified graphene;
[0014] The mass ratio of graphene oxide to phosphoric acid is 1:0.2-0.5;
[0015] The mass ratio of graphene oxide to polyethylene glycol is 1:0.8-1.2;
[0016] The hydrothermal temperature is 140°C to 150°C.
[0017] S4. Mix the purified liquid and the alkali, heat them, and add carbonate to react to obtain Li2CO3.
[0018] According to one technical solution of the roasting method technical solution of the present invention, at least the following beneficial effects are achieved:
[0019] The present invention adopts microwave-assisted hydrogen reduction to achieve efficient and selective reduction of nickel, cobalt and manganese in ternary cathode waste and fully separate them from lithium, thereby improving the separation effect of lithium and other metal elements.
[0020] In the present invention, after the reduction product is mixed with water, most of the metal elements such as nickel, cobalt and manganese have been reduced to metal elements or metal oxides, thereby achieving sufficient leaching of lithium elements and greatly reducing the content of impurity ions in the leachate; the present invention then mixes the leached phase with phosphorus-modified graphene to remove the impurity elements in the leached phase, further reducing the content of impurity ions;
[0021] In the present invention, the phosphorus-modified graphene is prepared under hydrothermal conditions using graphene oxide, phosphoric acid and polyethylene glycol as raw materials, and the graphene oxide and phosphoric acid are fully reacted to achieve phosphorylation of the graphene oxide surface; polyethylene glycol is then introduced into the surface of the phosphorylated graphene oxide, thereby greatly improving the dispersibility of the graphene material, thereby improving the ion removal effect of the phosphorus-modified graphene;
[0022] Finally, the present invention uses carbonate to achieve the precipitation of lithium ions, thereby preparing high-purity lithium carbonate; the present invention also uses magnetic separation to recover magnetic materials from leached residues, thereby improving the utilization rate of ternary positive electrode waste.
[0023] According to some embodiments of the present invention, the ternary material described in step S1 includes at least one of ternary waste materials, ternary recycled materials, ternary scraps, and ternary scrap materials.
[0024] According to some embodiments of the present invention, the mass fraction of lithium in the ternary cathode waste in step S1 is 3% to 6%.
[0025] According to some embodiments of the present invention, the mass fraction of manganese in the ternary cathode waste in step S1 is 10% to 30%.
[0026] According to some embodiments of the present invention, the mass fraction of nickel in the ternary cathode waste in step S1 is 20% to 40%.
[0027] According to some embodiments of the present invention, the mass fraction of cobalt in the ternary cathode waste in step S1 is 10% to 20%.
[0028] According to some embodiments of the present invention, the microwave reduction time is 30 min to 50 min.
[0029] According to some embodiments of the present invention, the flow rate of the hydrogen is 5 L / min to 10 L / min.
[0030] According to some embodiments of the present invention, the pressure of the hydrogen is 0.3 MPa to 0.4 MPa.
[0031] According to some embodiments of the present invention, the solid-liquid ratio of the reducing substance to water is 1 g: 15 mL to 20 mL.
[0032] According to some embodiments of the present invention, the reaction temperature in step S2 is 20°C to 30°C.
[0033] According to some embodiments of the present invention, the reaction time in step S2 is 1 h to 2 h.
[0034] According to some embodiments of the present invention, the magnetic field strength of the magnetic separation is 200KA / cm to 300KA / cm.
[0035] According to some embodiments of the present invention, the volume mass ratio of the leached phase to the phosphorus-modified graphene is 1L:100mg-200mg.
[0036] According to some embodiments of the present invention, the purification temperature in step S3 is 30°C to 40°C.
[0037] According to some embodiments of the present invention, the purification time in step S3 is 1 h to 2 h.
[0038] According to some embodiments of the present invention, the hydrothermal time is 6 h to 9 h.
[0039] According to some embodiments of the present invention, the number average molecular weight of the polyethylene glycol is 86,000 to 22,000.
[0040] According to some embodiments of the present invention, the polyethylene glycol is PEG-20000 or PEG-10000.
[0041] According to some embodiments of the present invention, the heating temperature in step S4 is 50°C to 90°C.
[0042] According to some embodiments of the present invention, the base in step S4 is sodium hydroxide or potassium hydroxide.
[0043] According to some embodiments of the present invention, the pH after heating in step S4 is 9-11.
[0044] According to some embodiments of the present invention, the carbonate is at least one of sodium carbonate or potassium carbonate. DETAILED DESCRIPTION
[0045] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0046] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0047] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0048] The method provided by the embodiment of the present invention grinds the waste ternary material into powder, so that it can be fully contacted with hydrogen and can be evenly heated under microwave radiation. Microwave treatment can reduce the activation energy of chemical reactions to a certain extent, reduce the reduction smelting temperature, and achieve efficient reduction at a relatively low temperature.
[0049] Microwave radiation penetrates and heats uniformly within the volume range at the same time, and can quickly heat up without causing surface overheating. During the reaction process, microwave irradiation does not require heat transfer and directly heats the material, which can achieve rapid, accurate and uniform heating of waste ternary materials.
[0050] In the embodiment of the present invention, the mass fraction of lithium in the waste ternary material is 4.32%, the mass fraction of nickel is 29.62%, the mass fraction of manganese is 11.21%, and the mass fraction of cobalt is 17.42%.
[0051] In the embodiment of the present invention, the graphene oxide is XF002-2 (sheet diameter: 0.5 μm to 5 μm, thickness: 0.8 nm to 1.2 nm) produced by Pioneer Nano.
[0052] Example 1
[0053] This embodiment is a combined recovery method of ternary materials, which consists of the following steps:
[0054] S1. Grind the ternary cathode waste into powder, introduce hydrogen (the flow rate of hydrogen is 8 L / min; the pressure of hydrogen is 0.35 MPa), mix well, and then perform microwave reduction at 600° C. to obtain a reduced product;
[0055] The microwave power is 2kW, the microwave frequency is 1.5GHZ, and the microwave reduction time is 40min;
[0056] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 25° C.; the reaction time in step S2 is 1.5 h), and then filtering to obtain leached residue and leached phase;
[0057] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 240KA / cm) to separate and recover nickel, cobalt and manganese;
[0058] S3, purifying the mixture of the leached phase and the phosphorus-modified graphene (the volume mass ratio of the leached phase to the phosphorus-modified graphene is 1 L: 150 mg) (the purification temperature in step S3 is 35° C.; the purification time in step S3 is 1.5 h) to obtain a purified solution;
[0059] The preparation method of phosphorus-modified graphene consists of the following steps:
[0060] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-10000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0061] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.4;
[0062] The mass ratio of graphene oxide and polyethylene glycol is 1:1;
[0063] The hydrothermal temperature is 145°C and the hydrothermal time is 7h.
[0064] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0065] Example 2
[0066] This embodiment is a combined recovery method of ternary materials, which consists of the following steps:
[0067] S1. Grind the ternary cathode waste into powder, introduce hydrogen (hydrogen flow rate is 10L / min; hydrogen pressure is 0.4MPa), mix well, and then perform microwave reduction at 550°C to obtain a reduced product;
[0068] The microwave power is 3kW, the microwave frequency is 1.5GHZ, and the microwave reduction time is 40min;
[0069] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 30° C.; the reaction time in step S2 is 1 h), and then filtering to obtain leached residue and leached phase;
[0070] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 300KA / cm) to separate and recover nickel, cobalt and manganese;
[0071] S3, purifying after mixing the leached phase and phosphorus-modified graphene (the volume mass ratio of the leached phase and the phosphorus-modified graphene is 1L:100mg) (the purification temperature in step S3 is 40°C; the purification time in step S3 is 1h) to obtain a purified solution;
[0072] The preparation method of phosphorus-modified graphene consists of the following steps:
[0073] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-20000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0074] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.5;
[0075] The mass ratio of graphene oxide to polyethylene glycol is 1:1.1;
[0076] The hydrothermal temperature was 140°C and the hydrothermal time was 9 h.
[0077] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0078] Example 3
[0079] This embodiment is a combined recovery method of ternary materials, which consists of the following steps:
[0080] S1. Grind the ternary cathode waste into powder, introduce hydrogen (the flow rate of hydrogen is 5 L / min; the pressure of hydrogen is 0.3 MPa), mix well, and then perform microwave reduction at 650°C to obtain a reduced product;
[0081] The microwave power was 2.4 kW, the microwave frequency was 1.2 GHZ, and the microwave reduction time was 40 min.
[0082] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g:15; the reaction temperature in step S2 is 25° C.; the reaction time in step S2 is 1.5 h.), and then filtering to obtain leached residue and leached phase;
[0083] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 250KA / cm) to separate and recover nickel, cobalt and manganese;
[0084] S3, purifying after mixing the leached phase and phosphorus-modified graphene (the volume mass ratio of the leached phase and the phosphorus-modified graphene is 1L:200mg) (the purification temperature in step S3 is 40°C; the purification time in step S3 is 1h) to obtain a purified solution;
[0085] The preparation method of phosphorus-modified graphene consists of the following steps:
[0086] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-10000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0087] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.4;
[0088] The mass ratio of graphene oxide to polyethylene glycol is 1:1.2;
[0089] The hydrothermal temperature is 150°C and the hydrothermal time is 6 hours.
[0090] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0091] Example 4
[0092] This embodiment is a combined recovery method of ternary materials, which consists of the following steps:
[0093] S1. Grind the ternary cathode waste into powder, introduce hydrogen (the flow rate of hydrogen is 9 L / min; the pressure of hydrogen is 0.34 MPa), mix well, and then perform microwave reduction at 700° C. to obtain a reduced product;
[0094] The microwave power is 2kW, the microwave frequency is 1GHZ, and the microwave reduction time is 40min;
[0095] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 18 mL; the reaction temperature in step S2 is 25° C.; the reaction time in step S2 is 1 h), and then filtering to obtain leaching residue and leaching phase;
[0096] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0097] S3, purifying the mixture of the leached phase and the phosphorus-modified graphene (the volume mass ratio of the leached phase to the phosphorus-modified graphene is 1 L: 180 mg) (the purification temperature in step S3 is 30° C.; the purification time in step S3 is 2 h) to obtain a purified solution;
[0098] The preparation method of phosphorus-modified graphene consists of the following steps:
[0099] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-10000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0100] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.3;
[0101] The mass ratio of graphene oxide to polyethylene glycol is 1:0.9;
[0102] The hydrothermal temperature is 140°C, and the hydrothermal time is 9 hours.
[0103] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0104] Example 5
[0105] This embodiment is a combined recovery method of ternary materials, which consists of the following steps:
[0106] S1. Grind the ternary cathode waste into powder, introduce hydrogen (hydrogen flow rate is 5 L / min; hydrogen pressure is 0.3 MPa), mix well, and then perform microwave reduction at 550° C. to obtain a reduced product;
[0107] The microwave power is 1kW, the microwave frequency is 1GHZ, and the microwave reduction time is 40min;
[0108] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 20° C.; the reaction time in step S2 is 2 h), and then filtering to obtain leached residue and leached phase;
[0109] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0110] S3, purifying after mixing the leached phase and phosphorus-modified graphene (the volume mass ratio of the leached phase and the phosphorus-modified graphene is 1L:100mg) (the purification temperature in step S3 is 30°C; the purification time in step S3 is 2h) to obtain a purified solution;
[0111] The preparation method of phosphorus-modified graphene consists of the following steps:
[0112] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-10000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0113] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.2;
[0114] The mass ratio of graphene oxide to polyethylene glycol is 1:0.8;
[0115] The hydrothermal temperature is 140°C and the hydrothermal time is 6 hours.
[0116] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0117] Comparative Example 1
[0118] This comparative example is a combined recovery method of ternary materials, which consists of the following steps:
[0119] S1. Grind the ternary cathode waste into powder, introduce hydrogen (the flow rate of hydrogen is 5 L / min; the pressure of hydrogen is 0.3 MPa), mix well, and then perform microwave reduction at 500° C. to obtain a reduced product;
[0120] The microwave power is 1kW, the microwave frequency is 1GHZ, and the microwave reduction time is 40min;
[0121] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 20° C.; the reaction time in step S2 is 2 h), and then filtering to obtain leached residue and leached phase;
[0122] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0123] S3, purifying after mixing the leached phase and phosphorus-modified graphene (the volume mass ratio of the leached phase and the phosphorus-modified graphene is 1L:100mg) (the purification temperature in step S3 is 30°C; the purification time in step S3 is 2h) to obtain a purified solution;
[0124] The preparation method of phosphorus-modified graphene consists of the following steps:
[0125] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-8000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0126] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.15;
[0127] The mass ratio of graphene oxide to polyethylene glycol is 1:0.8;
[0128] The hydrothermal temperature is 140°C and the hydrothermal time is 6 hours.
[0129] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0130] Comparative Example 2
[0131] This comparative example is a combined recovery method of ternary materials, which consists of the following steps:
[0132] S1. Grind the ternary cathode waste into powder, introduce hydrogen (the flow rate of hydrogen is 5 L / min; the pressure of hydrogen is 0.3 MPa), mix well, and then perform microwave reduction at 450°C to obtain a reduced product;
[0133] The microwave power is 1kW, the microwave frequency is 1GHZ, and the microwave reduction time is 40min;
[0134] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 20° C.; the reaction time in step S2 is 2 h), and then filtering to obtain leached residue and leached phase;
[0135] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0136] S3, purifying after mixing the leached phase and phosphorus-modified graphene (the volume mass ratio of the leached phase and the phosphorus-modified graphene is 1L:100mg) (the purification temperature in step S3 is 30°C; the purification time in step S3 is 2h) to obtain a purified solution;
[0137] The preparation method of phosphorus-modified graphene consists of the following steps:
[0138] Graphene oxide, phosphoric acid solution (85% by mass), polyethylene glycol (PEG-10000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0139] The mass ratio of graphene oxide and phosphoric acid solution is 1:0.1;
[0140] The mass ratio of graphene oxide to polyethylene glycol is 1:0.5;
[0141] The hydrothermal temperature is 140°C and the hydrothermal time is 6 hours.
[0142] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0143] Comparative Example 3
[0144] This comparative example is a combined recovery method of ternary materials, which consists of the following steps:
[0145] S1. Grind the ternary cathode waste into powder, introduce hydrogen (hydrogen flow rate is 5 L / min; hydrogen pressure is 0.3 MPa), mix well, and then perform microwave reduction at 550° C. to obtain a reduced product;
[0146] The microwave power is 1kW, the microwave frequency is 1GHZ, and the microwave reduction time is 20min;
[0147] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 20° C.; the reaction time in step S2 is 2 h), and then filtering to obtain leached residue and leached phase;
[0148] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0149] S3, purifying after mixing the leached phase and the modified graphene (the volume mass ratio of the leached phase and the modified graphene is 1L:100mg) (the purification temperature in step S3 is 30°C; the purification time in step S3 is 2h) to obtain a purified solution;
[0150] The preparation method of modified graphene consists of the following steps:
[0151] Graphene oxide, polyethylene glycol (PEG-10000) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain modified graphene;
[0152] The mass ratio of graphene oxide to polyethylene glycol is 1:0.8;
[0153] The hydrothermal temperature is 140°C and the hydrothermal time is 6 hours.
[0154] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0155] Comparative Example 4
[0156] This comparative example is a combined recovery method of ternary materials, which consists of the following steps:
[0157] S1. Grind the ternary cathode waste into powder, introduce hydrogen (hydrogen flow rate is 5 L / min; hydrogen pressure is 0.3 MPa), mix well, and then perform microwave reduction at 550° C. to obtain a reduced product;
[0158] The microwave power is 1kW, the microwave frequency is 1GHZ, and the microwave reduction time is 40min;
[0159] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 20° C.; the reaction time in step S2 is 2 h), and then filtering to obtain leached residue and leached phase;
[0160] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0161] S3, purifying after mixing the leached phase and phosphorus-modified graphene (the volume mass ratio of the leached phase and the phosphorus-modified graphene is 1L:100mg) (the purification temperature in step S3 is 30°C; the purification time in step S3 is 2h) to obtain a purified solution;
[0162] The preparation method of phosphorus-modified graphene consists of the following steps:
[0163] Graphene oxide, phosphoric acid solution (85% by mass) and water (the mass ratio of graphene oxide to water is 1 g: 200 mL) are mixed and hydrothermally treated to obtain phosphorus-modified graphene;
[0164] The mass ratio of graphene oxide to phosphoric acid solution is 1:0.2;
[0165] The hydrothermal temperature is 140°C and the hydrothermal time is 6 hours.
[0166] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0167] Comparative Example 5
[0168] This comparative example is a combined recovery method of ternary materials, which consists of the following steps:
[0169] S1. Grind the ternary cathode waste into powder, introduce hydrogen (hydrogen flow rate is 5 L / min; hydrogen pressure is 0.3 MPa), mix well, and then perform microwave reduction at 550° C. to obtain a reduced product;
[0170] The microwave power is 1kW, the microwave frequency is 1GHZ, and the microwave reduction time is 40min;
[0171] S2, placing the reduced product in water for sufficient reaction (the solid-liquid ratio of the reduced product to water is 1 g: 20 mL; the reaction temperature in step S2 is 20° C.; the reaction time in step S2 is 2 h), and then filtering to obtain leached residue and leached phase;
[0172] The leached residue is magnetically separated (the magnetic field strength of the magnetic separation is 200KA / cm) to separate and recover nickel, cobalt and manganese;
[0173] S3, purifying after mixing the leached phase and graphene oxide (the volume mass ratio of the leached phase and graphene oxide is 1L:100mg) (the purification temperature in step S3 is 30°C; the purification time in step S3 is 2h) to obtain a purified solution;
[0174] S4. Mix the purified liquid and alkali (sodium hydroxide) and heat them (heating temperature is 80° C., pH after heating is 11), and add carbonate (sodium carbonate) to react to obtain Li2CO3; separate the solid and liquid, collect the solid phase, and dry it.
[0175] The recovery rate of metallic lithium was calculated based on the mass and purity of the lithium carbonate obtained in Examples 1 to 5 and Comparative Examples 1 to 5. The results are shown in Table 1.
[0176] Table 1 The recovery rate of metallic lithium and the purity of lithium carbonate in Examples 1 to 5 of the present invention and Comparative Examples 1 to 5
[0177] - Recovery rate of metallic lithium (%) Purity of lithium carbonate (%) Example 1 95.81 98.6 Example 2 95.47 98.3 Example 3 96.19 97.8 Example 4 95.88 97.1 Example 5 94.01 96.9 Comparative Example 1 88.89 91.3 Comparative Example 2 79.36 90.7 Comparative Example 3 69.15 88.4 Comparative Example 4 93.78 85.6 Comparative Example 5 93.85 83.2
[0178] In summary, the present invention adopts microwave-enhanced hydrogen reduction to achieve efficient reduction of nickel, cobalt and manganese in ternary positive electrode waste and full separation from lithium, thereby improving the separation effect of lithium from other metal elements; in the present invention, after the reduced product is mixed with water, most of the metal elements such as nickel, cobalt and manganese have been reduced to metal elements or metal oxides, thereby achieving full leaching of lithium, greatly reducing the content of impurity ions in the leachate; the present invention then mixes the leached phase with phosphorus-modified graphene to further remove the impurity elements in the leached phase. Elements; in the present invention, phosphorus-modified graphene is prepared under hydrothermal conditions using graphene oxide, phosphoric acid and polyethylene glycol as raw materials, and the graphene oxide and phosphoric acid fully react to achieve phosphorylation of the graphene oxide surface; then polyethylene glycol is introduced to the surface of phosphorylated graphene oxide, thereby greatly improving the dispersibility of the graphene material, thereby improving the ion removal effect of the phosphorus-modified graphene; the present invention finally uses carbonate to achieve the precipitation of lithium ions, thereby obtaining high-purity lithium carbonate; the present invention also uses magnetic separation to recover magnetic materials from leached residues, thereby improving the utilization rate of ternary positive electrode waste. This application uses a pyrometallurgical and hydrometallurgical method to jointly treat waste ternary materials, and at the same time combines the use of impurity removers. Through a process with simple steps, easy operation and easy control, efficient recovery of waste ternary materials can be achieved, with high economic benefits, safety and environmental protection, and significantly reduced three waste emissions compared to pure pyrometallurgical method, pure hydrometallurgical method and general combined process, and can obtain high-purity lithium carbonate, with significant economic benefits.
[0179] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A combined recovery method of ternary materials, characterized in that: include: S1. Grind the ternary cathode waste into powder, introduce hydrogen into the powder and mix evenly, then perform microwave reduction at 550°C to 700°C to obtain a reduced product; The power of the microwave is 1 kW to 3 kW, and the frequency of the microwave is 1 GHZ to 1.5 GHZ; S2, placing the reduced product into water for full reaction, and then filtering to obtain leaching residue and leaching phase; Magnetic separation of nickel and / or cobalt and / or manganese from the leached residue for subsequent recovery; S3, purifying the leached phase and the phosphorus-modified graphene after mixing to obtain a purified solution; The method for preparing the phosphorus-modified graphene comprises the following steps: The graphene oxide, phosphoric acid solution, polyethylene glycol and water are mixed and then hydrothermally treated to obtain phosphorus-modified graphene; The mass ratio of graphene oxide to phosphoric acid is 1:0.2-0.5; The mass ratio of graphene oxide to polyethylene glycol is 1:0.8-1.2; The hydrothermal temperature is 140°C to 150°C; S4, mixing the purified liquid and the alkali, heating them, and adding carbonate to react to obtain Li2CO3; The reaction temperature in step S2 is 20°C to 30°C; The reaction time in step S2 is 1 h to 2 h.
2. The combined recovery method of ternary materials according to claim 1, characterized in that: The ternary material in step S1 includes at least one of ternary waste materials, ternary recycled materials, ternary scraps, and ternary scrap materials.
3. The combined recovery method of ternary materials according to claim 1, characterized in that: The solid-liquid ratio of the reducing substance to water is 1g:15mL~20mL.
4. The combined recovery method of ternary materials according to claim 1, characterized in that: The magnetic field strength of the magnetic separation is 200KA / cm~300KA / cm.
5. The combined recovery method of ternary materials as claimed in claim 1, characterized in that: The hydrothermal time is 6h~9h.
6. The combined recovery method of ternary materials according to claim 1, characterized in that: The number average molecular weight of the polyethylene glycol is 86000-22000.
7. The combined recovery method of ternary materials according to claim 1, characterized in that: The heating temperature in step S4 is 50°C to 90°C.
8. The combined recovery method of ternary materials according to claim 1, characterized in that: The alkali in step S4 is sodium hydroxide or potassium hydroxide.
9. The combined recovery method of ternary materials according to claim 1, characterized in that: The pH after heating in step S4 is 9-11.
10. The combined recovery method of ternary materials according to claim 1, characterized in that: The carbonate is at least one of sodium carbonate or potassium carbonate.
Citation Information
Cited By
A method for regenerating lithium battery waste
CN118563089B
Roasting method of lithium battery waste
CN120174193A