A copper electroplating process for circuit boards
By adding specific extracts to the plating solution to form an oxidation-resistant copper foil, the problem of oxidation of the circuit board in a humid environment is solved, the service life of the circuit board is extended and the conductive properties are maintained.
Patent Information
- Application Number
- CN202410217655.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-28
AI Technical Summary
The copper foil is prone to oxidation in a humid environment, resulting in a decrease in conductivity and a shortened life. It is difficult for the prior art to effectively prevent the oxidation of copper foil.
Using an electroplating copper process, the copper foil is placed in the base by configuring copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, mulberry parasitic extract, Eucalyptus blue leaf extract and Marxa vine extract in the electroplating solution. The formation of material plates has strong oxidation resistance and prevents oxidation.
It extends the service life of the circuit board and maintains good conductivity. Even if the paint film is damaged, the copper foil is not easy to oxidize, which significantly improves the durability of the circuit board.
Abstract
Description
Technical Field
[0001] The invention relates to the field of circuit board electroplating technology, in particular to a copper electroplating technology for a circuit board. Background Art
[0002] Circuit boards make circuits miniaturized and intuitive, and can be mass-produced to fix circuits, making them an indispensable part of existing electrical appliances.
[0003] Circuit boards are mainly made by covering an insulating substrate with copper foil to form a copper-clad laminate, and then printing circuits on the copper-clad laminate to form a circuit board with a fixed circuit. Therefore, the conductive performance of the circuit board is mainly achieved through the copper foil.
[0004] Copper is not easy to oxidize in a dry environment, but it oxidizes quickly in humid air. When the circuit board is in humid air, the circuit formed by the copper foil will oxidize, resulting in a decrease in the conductivity of the circuit. Therefore, it is usually necessary to coat the surface of the circuit board with paint to isolate the copper foil from oxygen and water vapor, thereby reducing the oxidation of the circuit in the circuit board.
[0005] However, in the actual production and use process, the paint film on the surface of the circuit board will be damaged due to friction or aging. When the paint film is damaged, the copper circuit in the circuit board will come into contact with the air, and under the action of oxygen and water vapor, copper oxidation will be caused, which will affect the performance of the circuit board and shorten the life of the circuit board. Therefore, there is still room for improvement. Summary of the invention
[0006] In order to prevent the circuit board from being easily oxidized and thus prolong its life, the present application provides a copper electroplating process for a circuit board.
[0007] The present application provides a copper electroplating process for a circuit board using the following technical solution:
[0008] A copper electroplating process for a circuit board comprises the following steps:
[0009] Step 1), prepare the plating solution:
[0010] The electroplating solution is prepared by mixing copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, a buffer, a mistletoe extract, a eucalyptus globulus leaf extract, a gymnema extract, and deionized water.
[0011] Step 2), immersing the substrate plate in an electroplating solution, applying power for electroplating, and obtaining an electroplated copper plate.
[0012] By adopting the above technical solution and configuring a special electroplating solution, the copper foil electroplated on the substrate board has good anti-oxidation properties. After the paint film coated on the circuit board is damaged, the copper foil is still not easy to oxidize, so that the circuit on the circuit board is not easy to oxidize, so that the circuit board can maintain good conductive properties for a longer time, and effectively extend the service life of the circuit board.
[0013] By adding mistletoe extract, eucalyptus globulus leaf extract and gymnema extract into the electroplating solution and dissolving the mistletoe extract, eucalyptus globulus leaf extract and gymnema extract in deionized water, the mistletoe extract, eucalyptus globulus leaf extract and gymnema extract will be incorporated into the copper foil during the process of copper being deposited on the substrate board due to electroplating, thereby protecting the copper foil, making it difficult for copper atoms to react with oxygen atoms and become oxidized, and making it difficult for the copper foil to be oxidized when directly exposed to humid air to affect the conductivity of the circuit, thereby effectively extending the service life of the circuit board.
[0014] Preferably, the mass ratio of the copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, wetting agent, buffer, mistletoe extract, eucalyptus globulus leaf extract and gymnema truncatum extract is 80-100:50-70:40-60:60-80:30-50:20-30:10-20:15-25.
[0015] By adopting the above technical scheme and specifically selecting the mass ratios of copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, wetting agent, buffer, mistletoe extract, eucalyptus globulus leaf extract and gymnema truncatum extract, the electroplating copper foil has a better effect, the copper foil is not easy to generate bubbles, and at the same time, the copper foil has higher antioxidant properties and is less likely to oxidize in humid air. The prepared circuit board can be used for a long time when the paint film is damaged, and the prepared circuit board has a longer life.
[0016] Preferably, the mass ratio of copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, wetting agent, buffer, mistletoe extract, eucalyptus globulus leaf extract, gymnema extract and deionized water is 80-100:50-70:40-60:60-80:30-50:20-30:10-20:15-25:1000.
[0017] By adopting the above technical scheme and specifically selecting the mass ratios of copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, wetting agent, buffer, mistletoe extract, eucalyptus globulus leaf extract, gymnema oleifera extract, and deionized water, the copper electroplating effect is better, the copper foil formed by electroplating has better antioxidant properties, and at the same time, material waste is reduced, thereby having higher economic value.
[0018] Preferably, the Herba Moriformis extract is a water-soluble extract.
[0019] By adopting the above technical scheme and specifically selecting the mistletoe extract as the water-soluble extract, the mistletoe extract can be well dispersed in the electroplating solution, the effect of modifying the electroplated copper foil is better, and the antioxidant performance of the electroplated copper foil is better improved.
[0020] Preferably, the Eucalyptus globulus leaf extract is a water-soluble extract.
[0021] By adopting the above technical solution and specifically selecting the eucalyptus globulus leaf extract as the water-soluble extract, the eucalyptus globulus leaf extract can be well dispersed in the electroplating solution and can better cooperate with other components, thereby achieving a better effect in improving the antioxidant properties of the electroplated copper foil.
[0022] Preferably, the Gymnema truncatum extract is a water-soluble extract.
[0023] By adopting the above technical scheme, by specifically selecting the gymnema extract as the water-soluble extract, the gymnema extract can be better dispersed in the electroplating solution, and can better cooperate with the mistletoe extract and the eucalyptus leaf extract to exert a better synergistic effect, thereby making the antioxidant performance of the electroplated copper higher and the life of the resulting circuit board longer.
[0024] Preferably, in step 2), during electroplating, the temperature is 22-25°C and the current density is 2-3A / dm 2 , the electroplating time is 18-22min.
[0025] By adopting the above technical solution and specifically selecting the temperature, current density and electroplating time during electroplating, the quality of electroplating is better, the thickness of the electroplated copper foil is more appropriate and the quality of the electroplated copper foil is better.
[0026] Preferably, the buffer is citric acid.
[0027] By adopting the above technical solution and specifically selecting citric acid as the buffer, the quality of the electroplating solution is better, the effect of electroplating copper foil is better, and the quality of the produced circuit board is higher.
[0028] In summary, this application has the following beneficial effects:
[0029] 1. Since the present application configures a special electroplating solution, the copper foil formed by electroplating has good anti-oxidation properties. After the paint film coated on the circuit board is damaged, the copper foil is still not easy to oxidize, so that the circuit board can maintain good conductive properties for a longer time, effectively extending the service life of the circuit board.
[0030] 2. In the present application, it is preferred to add mistletoe extract, eucalyptus globulus leaf extract and gymnema extract to the electroplating solution. During the process of copper deposition on the substrate board, the mistletoe extract, eucalyptus globulus leaf extract and gymnema extract will be incorporated into the copper foil, thereby protecting the copper foil, making it difficult for copper atoms to react with oxygen atoms and oxidize, thereby effectively extending the service life of the circuit board.
[0031] 3. In the present application, it is preferred that the copper foil formed by electroplating has good antioxidant properties, reduces material waste, and has high economic value by specifically selecting the mass ratio of copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, wetting agent, buffer, mistletoe extract, eucalyptus globulus leaf extract, gymnema extract, and deionized water. DETAILED DESCRIPTION
[0032] The present application is further described in detail below with reference to the embodiments.
[0033] Example 1
[0034] A copper electroplating process for a circuit board comprises the following steps:
[0035] Step 1), prepare the plating solution:
[0036] Weigh 80 g of copper sulfate, 50 g of copper chloride, 40 g of sodium thiosulfate, 60 g of potassium sulfate, 30 g of buffer, 20 g of mistletoe extract, 10 g of eucalyptus globulus leaf extract, 15 g of gymnema extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 75°C, rotate at 120 r / min, stir for 15 minutes, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0037] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 22°C and the current density is controlled to 2A / dm 2 , power is turned on for electroplating, the electroplating time is 22 minutes, after the electroplating is completed, the substrate board is taken out and naturally air-dried to obtain the electroplated copper board.
[0038] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0039] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0040] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0041] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0042] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0043] Among them, the mistletoe extract was purchased from Shaanxi Xintianyu Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0044] Among them, the eucalyptus globulus leaf extract was purchased from Xi'an Ruierli Bioengineering Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0045] Among them, the gymnema oleifera extract was purchased from Xi'an Youshuo Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0046] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0047] Example 2
[0048] A copper electroplating process for a circuit board comprises the following steps:
[0049] Step 1), prepare the plating solution:
[0050] Weigh 90 g of copper sulfate, 60 g of copper chloride, 50 g of sodium thiosulfate, 70 g of potassium sulfate, 40 g of buffer, 25 g of mistletoe extract, 15 g of eucalyptus globulus leaf extract, 20 g of gymnema extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 78°C, rotate at 120 r / min, stir for 18 min, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0051] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 23°C and the current density is controlled to 2.5A / dm 2 , power is turned on for electroplating, the electroplating time is 20 minutes, after the electroplating is completed, the substrate plate is taken out and naturally air-dried to obtain the electroplated copper plate.
[0052] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0053] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0054] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0055] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0056] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0057] Among them, the mistletoe extract was purchased from Shaanxi Xintianyu Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0058] Among them, the eucalyptus globulus leaf extract was purchased from Xi'an Ruierli Bioengineering Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0059] Among them, the gymnema oleifera extract was purchased from Xi'an Youshuo Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0060] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0061] Example 3
[0062] A copper electroplating process for a circuit board comprises the following steps:
[0063] Step 1), prepare the plating solution:
[0064] Weigh 100 g of copper sulfate, 70 g of copper chloride, 60 g of sodium thiosulfate, 80 g of potassium sulfate, 50 g of buffer, 30 g of mistletoe extract, 20 g of eucalyptus globulus leaf extract, 25 g of gymnema extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 80°C, rotate at 120 r / min, stir for 20 min, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0065] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and immerse the substrate plate completely in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 25°C and the current density is controlled to 3A / dm 2 , power is turned on for electroplating, the electroplating time is 22 minutes, after the electroplating is completed, the substrate board is taken out and naturally air-dried to obtain the electroplated copper board.
[0066] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0067] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0068] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0069] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0070] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0071] Among them, the mistletoe extract was purchased from Shaanxi Xintianyu Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0072] Among them, the eucalyptus globulus leaf extract was purchased from Xi'an Ruierli Bioengineering Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0073] Among them, the gymnema oleifera extract was purchased from Xi'an Youshuo Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0074] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0075] Comparative Example 1
[0076] A copper electroplating process for a circuit board comprises the following steps:
[0077] Step 1), prepare the plating solution:
[0078] Weigh 90 g of copper sulfate, 60 g of copper chloride, 50 g of sodium thiosulfate, 70 g of potassium sulfate, 40 g of buffer, 25 g of gallnut extract, 15 g of eucalyptus globulus leaf extract, 20 g of gymnema extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 78°C, rotate at 120 r / min, stir for 18 min, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0079] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 23°C and the current density is controlled to 2.5A / dm 2 , power is turned on for electroplating, the electroplating time is 20 minutes, after the electroplating is completed, the substrate plate is taken out and naturally air-dried to obtain the electroplated copper plate.
[0080] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0081] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0082] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0083] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0084] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0085] Among them, the gallnut extract was purchased from Xi'an Green Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0086] Among them, the eucalyptus globulus leaf extract was purchased from Xi'an Ruierli Bioengineering Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0087] Among them, the gymnema oleifera extract was purchased from Xi'an Youshuo Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0088] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0089] Comparative Example 2
[0090] A copper electroplating process for a circuit board comprises the following steps:
[0091] Step 1), prepare the plating solution:
[0092] Weigh 90 g of copper sulfate, 60 g of copper chloride, 50 g of sodium thiosulfate, 70 g of potassium sulfate, 40 g of buffer, 25 g of mistletoe extract, 15 g of rosemary extract, 20 g of gymnema extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 78°C, rotate at 120 r / min, stir for 18 min, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0093] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 23°C and the current density is controlled to 2.5A / dm 2 , power is turned on for electroplating, the electroplating time is 20 minutes, after the electroplating is completed, the substrate plate is taken out and naturally air-dried to obtain the electroplated copper plate.
[0094] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0095] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0096] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0097] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0098] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0099] Among them, the mistletoe extract was purchased from Shaanxi Xintianyu Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0100] Among them, rosemary extract was purchased from Shaanxi Yunsheng Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0101] Among them, the gymnema oleifera extract was purchased from Xi'an Youshuo Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0102] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0103] Comparative Example 3
[0104] A copper electroplating process for a circuit board comprises the following steps:
[0105] Step 1), prepare the plating solution:
[0106] Weigh 90 g of copper sulfate, 60 g of copper chloride, 50 g of sodium thiosulfate, 70 g of potassium sulfate, 40 g of buffer, 25 g of mistletoe extract, 15 g of eucalyptus globulus leaf extract, 20 g of grape seed extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 78°C, rotate at 120 r / min, stir for 18 min, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0107] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 23°C and the current density is controlled to 2.5A / dm 2 , power is turned on for electroplating, the electroplating time is 20 minutes, after the electroplating is completed, the substrate plate is taken out and naturally air-dried to obtain the electroplated copper plate.
[0108] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0109] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0110] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0111] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0112] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0113] Among them, the mistletoe extract was purchased from Shaanxi Xintianyu Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0114] Among them, the eucalyptus globulus leaf extract was purchased from Xi'an Ruierli Bioengineering Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0115] Among them, grape seed extract was purchased from Baoji Runmu Agricultural Development Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0116] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0117] Comparative Example 4
[0118] A copper electroplating process for a circuit board comprises the following steps:
[0119] Step 1), prepare the plating solution:
[0120] Weigh 90 g of copper sulfate, 60 g of copper chloride, 50 g of sodium thiosulfate, 70 g of potassium sulfate, 40 g of buffer, 25 g of gallnut extract, 15 g of rosemary extract, 20 g of grape seed extract, and 1000 g of deionized water, put them into a stirring kettle, heat to 78° C., rotate at 120 r / min, stir for 18 min, mix well, and naturally cool to room temperature to obtain an electroplating solution.
[0121] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 23°C and the current density is controlled to 2.5A / dm 2 , power is turned on for electroplating, the electroplating time is 20 minutes, after the electroplating is completed, the substrate plate is taken out and naturally air-dried to obtain the electroplated copper plate.
[0122] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0123] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0124] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0125] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0126] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0127] Among them, the gallnut extract was purchased from Xi'an Green Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0128] Among them, rosemary extract was purchased from Shaanxi Yunsheng Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0129] Among them, grape seed extract was purchased from Baoji Runmu Agricultural Development Co., Ltd., a water-soluble extract with an extraction ratio of 10:1.
[0130] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0131] Comparative Example 5
[0132] A copper electroplating process for a circuit board comprises the following steps:
[0133] Step 1), prepare the plating solution:
[0134] Weigh 90 g of copper sulfate, 60 g of copper chloride, 50 g of sodium thiosulfate, 70 g of potassium sulfate, 40 g of buffer, 25 g of benzyl acetone, 15 g of 1,4-butynediol, 20 g of polyhydroxypropyl dimethyl ammonium chloride, and 1000 g of deionized water, put them into a stirring kettle, heat to 78°C, rotate at 120 r / min, stir for 18 min, mix well, and cool naturally to room temperature to obtain an electroplating solution.
[0135] Step 2), inject the electroplating solution into the electroplating tank, insert the anode plate into the electroplating solution, clamp the substrate plate that has completed chemical copper plating on the tool, and completely immerse the substrate plate in the electroplating solution. The anode plate is connected to the positive electrode, and the substrate plate is connected to the negative electrode. The electroplating solution is kept at a constant temperature of 23°C and the current density is controlled to 2.5A / dm 2 , power is turned on for electroplating, the electroplating time is 20 minutes, after the electroplating is completed, the substrate plate is taken out and naturally air-dried to obtain the electroplated copper plate.
[0136] Wherein, copper sulfate is copper sulfate pentahydrate, which is commercially available, CAS number: 7758-98-7.
[0137] Wherein, the cupric chloride is cupric chloride dihydrate, which is commercially available, CAS number: 10125-13-0.
[0138] Wherein, sodium thiosulfate is commercially available, CAS number: 7772-98-7.
[0139] Wherein, potassium sulfate is commercially available, CAS number: 7778-80-5.
[0140] The buffer is citric acid monohydrate, which is commercially available with a CAS number of 5949-29-1.
[0141] Among them, benzyl acetone was purchased from Jinan Xinqidian Chemical Co., Ltd.
[0142] Among them, 1,4-butynediol was purchased from Wuxi Jingke Chemical Co., Ltd.
[0143] Among them, polyhydroxypropyl dimethyl ammonium chloride was purchased from Langfang Jifang Technology Co., Ltd.
[0144] Among them, the anode plates were purchased from Baoji Zhiming Special Metal Co., Ltd., titanium anode plates.
[0145] Experiment 1
[0146] The electroplated copper plates prepared in the embodiments and comparative examples were placed in a constant temperature and humidity chamber at a constant temperature of 40±1°C and a relative humidity of 80±1%, with ventilation maintained, for 30 days, and then the surface oxidation of the electroplated copper plates was observed.
[0147] The specific test data of Experiment 1 are as follows:
[0148] Example 1: The surface is bright and has no oxidation.
[0149] Example 2: The surface is bright and has no oxidation.
[0150] Example 3: The surface is bright and has no oxidation.
[0151] Comparative Example 1: The surface is dull and black, with verdigris and oxidation appearing locally.
[0152] Comparative Example 2: The surface is dull and black, with verdigris and oxidation appearing in some areas.
[0153] Comparative Example 3: The surface is dull and black, with verdigris and oxidation appearing in some areas.
[0154] Comparative Example 4: The surface is dull and black, verdigris appears over a large area, and oxidation is quite serious.
[0155] Comparative Example 5: The surface is dull and black, with verdigris and oxidation appearing in some areas.
[0156] According to the comparison of the test data of Experiment 1, it can be obtained that the electroplated copper plates prepared in each embodiment do not show any oxidation phenomenon when stored under high humidity and high temperature conditions for 90 days, and the anti-oxidation performance is significantly higher than that of each comparative example.
[0157] In Comparative Examples 1-5, due to the destruction of the compound system of the mistletoe extract, eucalyptus leaf extract, and gymnema oleifera extract, the antioxidant performance improvement effect of the electroplated copper plate decreased significantly, causing the circuit board to oxidize quickly after the paint film was damaged, and the life of the circuit board was short.
[0158] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A copper electroplating process for a circuit board, characterized in that: The following steps are involved: Step 1), prepare the plating solution: The electroplating solution is prepared by mixing copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, a buffer, a mistletoe extract, a eucalyptus globulus leaf extract, a gymnema extract, and deionized water. Step 2), immersing the substrate plate in an electroplating solution, applying electricity for electroplating, and obtaining an electroplated copper plate; The mistletoe extract was purchased from Shaanxi New Horizon Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:1; The eucalyptus globulus leaf extract was purchased from Xi'an Ruierli Bioengineering Co., Ltd., a water-soluble extract, with an extraction ratio of 10:1; The gymnema oleifera extract was purchased from Xi'an Youshuo Biotechnology Co., Ltd., a water-soluble extract with an extraction ratio of 10:
1.
2. The copper electroplating process for a circuit board according to claim 1, characterized in that: The mass ratio of the copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, buffer, mistletoe extract, eucalyptus globulus leaf extract and gymnema truncatum extract is 80-100: 50-70: 40-60: 60-80: 30-50: 20-30: 10-20: 15-25.
3. The copper electroplating process for a circuit board according to claim 2, characterized in that: The mass ratio of copper sulfate, copper chloride, sodium thiosulfate, potassium sulfate, buffer, mistletoe extract, eucalyptus globulus leaf extract, gymnema extract and deionized water is 80-100:50-70:40-60:60-80:30-50:20-30:10-20:15-25:1000.
4. The copper electroplating process for a circuit board according to claim 1, characterized in that: In step 2), during electroplating, the temperature is 22-25°C and the current density is 2-3A / dm 2 , the electroplating time is 18-22min.
5. The copper electroplating process for a circuit board according to claim 1, characterized in that: The buffer is citric acid.