A method for controlling van der Waals gap and semiconductor device

By using the method of saturated steam and physical lamination of the precursor solution in the van der Waals gap, the problem of nanoscale van der Waals gap control is solved, the universality of material gaps and component regulation is achieved, and the application range of functional devices is expanded.

CN117877985BActive Publication Date: 2024-11-08HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311674582.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-07
Publication Date
2024-11-08
Estimated Expiration
2043-12-07

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control and regulate the van der Waals gap at the nanoscale. Traditional electrochemical intercalation technology is damaged to the electrical characteristics of materials and lacks universality, so it cannot be widely used in different material systems.

Method used

By generating different grades of precursor solution saturated steam, the target material is pre-adsorbed under saturated steam, and combined with physical lamination to form a van der Waals gap with controllable size, avoiding the formation of chemical bonds with the material.

Benefits of technology

It realizes universal control and component customization of Van der Waals gaps, maintains the intrinsic properties of the material, is suitable for materials of different dimensions and structures, and expands the application prospects of functional devices, including water filtration, ion screening and pressure sensing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117877985B_ABST
    Figure CN117877985B_ABST
Patent Text Reader

Abstract

The present invention provides a method for controlling a van der Waals gap, the method comprising the following steps: step 1, generating saturated steam using a precursor solution; step 2, placing a first material in saturated steam for molecular / ion adsorption; step 3, physically laminating the first material with a second material to form a van der Waals gap, the size of which is controlled by the saturated steam in which the first material is adsorbed. The present invention utilizes the difference in surface adsorption of materials under different levels of saturated steam, combined with subsequent physical lamination, to form a series of van der Waals gaps of varying sizes and compositions, the van der Waals gaps being able to be formed in two-dimensional (2D) / 2D materials, 2D / three-dimensional (3D) materials, 3D / 3D materials and artificial superlattice materials, and having a high degree of universality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor technology, especially the field of materials and semiconductor devices, and specifically relates to a universal method for nanoscale regulation of van der Waals gaps of materials of different dimensions and filling of multiple gap components. Background Art

[0002] The development of van der Waals technology has injected new vitality into the development of 2D materials. People can use this technology to assemble a variety of different 2D atomic crystals to form van der Waals heterostructures and superlattices.

[0003] As a derivative of van der Waals technology, nanoscale van der Waals gaps have become a research hotspot. First, manipulating van der Waals gaps can effectively modulate the interlayer distance, phase composition, electronic and optical properties of 2D materials. Second, designing van der Waals gaps in van der Waals structures can obtain a variety of functional devices with customized performance. At the same time, nanoscale van der Waals gaps are considered to be the most useful tool for studying extreme-scale material science, especially for the size of a single or a few atoms or molecules. People have discovered special phenomena at extreme sizes such as nanocapillary condensation, "ballistic" gas transport, and abrupt dielectric properties. In addition, for extremely small van der Waals gaps (subnanometer), its diameter can be smaller than the diameter of the smallest hydrated ion, so it can be used as a selective permeation pore, which has great potential in water filtration, molecular / ion separation, and seawater desalination.

[0004] However, controlling the van der Waals gap at the nanoscale has always been a technical challenge. This is because, once the van der Waals interaction is established, the size of the van der Waals gap is difficult to change, and its size depends solely on the lowest potential of the van der Waals interaction and the intrinsic properties of the atoms involved. So far, the strategy to open such a van der Waals gap still relies on traditional electrochemical intercalation technology, by which the host particles are driven to be inserted into the host material. However, the introduced organic macromolecules or alkali metal ions severely damage the electrical properties of the host material and have poor structural stability. Moreover, this method not only has insufficient control over the gap size, but can only be applied to characteristic material systems.

[0005] Although some conceptual prototypes and interesting science about the van der Waals gap have been reported, a universal method to open the van der Waals gap has not yet been achieved. Summary of the invention

[0006] The purpose of the present invention is to address the deficiencies of the prior art and provide a universal method for controlling the van der Waals gap, thereby achieving the creation, size regulation and gap composition customization of the van der Waals gap.

[0007] The method provided by the present invention generates saturated vapor of precursor solutions of different levels, and the target material is pre-adsorbed on the surface under the saturated vapor, and is physically laminated with another material, so that a van der Waals gap with controllable size can be assembled.

[0008] The technical solution adopted by the present invention is specifically as follows:

[0009] In a first aspect, the present invention provides a method for controlling a van der Waals gap, the method comprising the following steps:

[0010] Step 1, generating saturated steam using a precursor solution;

[0011] Step 2, placing the first material in saturated steam for molecular and / or ionic adsorption;

[0012] Step three, physically laminating the first material and the second material to form a van der Waals gap, wherein the size of the gap is controlled by the saturated steam in which the first material is adsorbed.

[0013] Preferably, the precursor solution is pure water or an aqueous solution containing different molecules and / or ions.

[0014] Preferably, in the step 1, the saturated steam is standard saturated steam, and the pressure of the saturated steam is controlled by the heating temperature of the solution.

[0015] Preferably, the size of the gap is controlled by the temperature of the saturated steam in which the first material is adsorbed.

[0016] Preferably, in step 1, the level of the saturated steam is controlled by the heating temperature of the solution.

[0017] Preferably, in step 2, the first material is a 2D and / or 3D material.

[0018] Preferably, the thickness of the first material is greater than 8 nm, which ensures that the adsorbed droplets can be uniformly squeezed to form a uniform van der Waals gap.

[0019] In a second aspect, the present invention provides a MoS 2 Homojunction, the MoS 2 The homojunction is prepared according to any one of claims 1 to 5, wherein the first material and the second material are MoS 2 .

[0020] Preferably, the MoS 2 The gap size of the homojunction is 0.55nm-5.36nm.

[0021] In a third aspect, the present invention provides a 2D / 3D heterojunction, wherein the 2D / 3D heterojunction is prepared according to the above method, and the first material and the second material are 2D and / or 3D materials.

[0022] In a fourth aspect, the present invention provides a multilayer MoS 2 Superlattice structure, the multilayer MoS 2 The superlattice structure is prepared according to the above method, wherein the first material and the second material are MoS 2 , the multilayer MoS 2 The gap size of each layer of the superlattice structure can be controlled.

[0023] In a fifth aspect, the present invention provides a MoS 2 / iodide ion solution gap / MoS 2 Structure, the MoS 2 / iodide ion solution gap / MoS 2 The structure is prepared according to the above method, wherein the first material and the second material are MoS 2 , the precursor solution is an iodine ion solution.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The present invention uses the surface pre-adsorption of materials in saturated molecular / ionic vapor as a means, combined with subsequent physical lamination, to form van der Waals gaps. The surface adsorption involved is physical adsorption, and no chemical bond is formed with the material, thereby avoiding the influence on the intrinsic properties of the material.

[0026] (2) The method for controlling the van der Waals gap described in the present invention is highly universal and does not need to consider the properties of the material. The method can be extended to materials and structures of different dimensions, including 2D / 2D homogeneous structures, 2D / 2D heterogeneous structures, 2D / 3D heterogeneous structures, artificial superlattice structures, etc. At the same time, the components in the gap can also be customized according to different adsorption, including different molecules and ions.

[0027] (3) The present invention can realize a variety of new principle devices and has broad application prospects. Different gap components and sizes can effectively modulate the properties of materials, for example, MoS 2 / van der Waals gap / MoS 2 It shows the characteristics of a diode. At the same time, ultra-small van der Waals gaps are expected to achieve water filtration, ion screening, seawater desalination, etc.; large van der Waals gaps are expected to achieve pressure sensing, etc.

[0028] (4) The method for controlling the van der Waals gap proposed in the present invention is simple, effective, universal and controllable. The formed van der Waals gap can effectively modulate the properties of the material and realize a variety of functional devices based on new principles. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 A schematic diagram of a saturated steam generating adsorption device provided by the present invention;

[0030] Figure 2 The saturated vapor pressure-temperature relationship diagram of pure water provided by the present invention;

[0031] Figure 3 A schematic diagram of a method for controlling the van der Waals gap provided by the present invention;

[0032] Figure 4 A series of MoS with varying van der Waals gaps prepared by the present invention 2 Electron micrograph of homogeneous structure;

[0033] Figure 5 The present invention uses pure water as a precursor solution and MoS 2 Gap height-temperature relationship diagram extracted as a standard adsorption object;

[0034] Figure 6 Schematic diagram of a series of van der Waals gap structures formed by materials of different types and dimensions prepared in the present invention;

[0035] Figure 7 The MoS prepared by the present invention 2 / Electron microscope image of the conceptual structure of the interstitial superlattice;

[0036] Figure 8 The MoS prepared by the present invention 2 / iodide ion solution gap / MoS 2 Electron micrograph of the structure and the corresponding elemental spectrum.

[0037] The reference numerals in the drawings are: 1-container, 2-water, 3-thermometer, 4-heating plate, 5-first material, 6-saturated steam, 7-precursor solution. DETAILED DESCRIPTION

[0038] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.

[0040] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0041] Embodiment 1

[0042] Embodiment 1 of the present invention provides a method for controlling the van der Waals gap. Figure 1 and Figure 2 , specifically including the following steps:

[0043] Step 1: using a precursor solution 7 to generate saturated steam 6.

[0044] Step 1 specifically includes: heating a closed container partially filled with the precursor solution at a constant temperature to achieve temperature equilibrium and generate constant saturated steam 6.

[0045] like Figure 1 As shown, Figure 1 (b) Figure 1 In the embodiment of the present invention, in order to obtain saturated steam 6, a closed container 1 with a small opening on the top is heated in advance by a water bath, the closed container 1 is placed in water 2, a heating plate 4 is installed at the bottom, and a precursor solution 7 is contained in the closed container 1, and the liquid level of the precursor solution 7 in the closed container 1 is ensured to be at the same level as the liquid level of the external water bath 2.

[0046] Preferably, a thermometer 3 is placed in the water bath, and the required saturated steam 6 can be accurately controlled by controlling the temperature of the external water bath.

[0047] The precursor solution 7 may be pure water, an aqueous solution containing different molecules and / or ions, or other solutions. The saturated steam is standard saturated steam, and the pressure of the saturated steam is controlled by the heating temperature.

[0048] Step 2: placing the first material 5 in saturated steam 6 for molecular and / or ionic adsorption.

[0049] When the saturated steam 6 reaches a stable state under the water bath heating, the first material 5 is placed at the top opening of the sealed container 1 , thereby sealing the container 1 and placing the first material 5 in the saturated steam 6 .

[0050] The saturated steam 6 is composed of a large number of molecules and / or ions. When the first material 5 is placed in the saturated steam 6 for a fixed period of time, the first material 5 will absorb the molecules and / or ions in the saturated steam.

[0051] After the adsorption is completed, many droplets will be formed on the surface of the first material 5, among which large droplets are more likely to form at defect sites.

[0052] At the same time, the first material 5 has different adsorption levels for different levels of saturated steam 6. The adsorption capacity is related to the saturated steam pressure, which is controlled by temperature. Therefore, adjusting the temperature of the saturated steam 6 can directly control the amount of adsorption on the surface of the first material 5.

[0053] For pure water, its saturated vapor pressure and temperature satisfy the exponential relationship as follows Figure 2 As shown, Figure 2 The saturated vapor pressure-temperature relationship diagram of pure water provided by the present invention is as follows: Figure 2 As shown, the horizontal axis is temperature and the vertical axis is saturated vapor pressure. Figure 2 It can be seen that the higher the temperature, the greater the saturated vapor pressure, and the saturated vapor pressure is related to the surface adsorption capacity of the first material 5 .

[0054] Experiments have shown that the amount of adsorption on the surface of the first material 5 can be directly controlled by temperature.

[0055] Preferably, the adsorption process should be carried out in an oxygen-free water environment to avoid the influence of related impurities on the adsorption control.

[0056] according to Figure 2 As shown, the temperature of pure water is 20° C.-100° C. For other solutions, the adsorption scheme consistent with this embodiment can be adopted.

[0057] Preferably, the adsorption time is about 5 minutes.

[0058] Preferably, the first material 5 may be a 2D or 3D material. For a 2D material, its thickness should be greater than 8 nm, which ensures that the adsorbed droplets can be uniformly squeezed to form a uniform van der Waals gap.

[0059] Preferably, the first material 5 is placed on a substrate and then placed at the top opening of the sealed container 1 to facilitate subsequent alignment transfer and lamination.

[0060] Step three, physically laminating the first material 5 and the second material to form a van der Waals gap, wherein the size of the gap is controlled by the saturated steam in which the first material 5 is adsorbed.

[0061] like Figure 3 As shown, Figure 3 (a) is the adsorption process of the first material 5. The first material 5 after adsorption is quickly mounted on a mechanical arm equipped with a microscope, and then mechanically aligned and laminated with the second material to form a van der Waals gap structure, as shown in FIG. Figure 3 (b) and Figure 3 (c) is shown. The electron microscope image of the van der Waals gap after lamination is shown in Figure 3 (d) as shown.

[0062] Preferably, the adsorbed first material 5 should be aligned and laminated in a short time to ensure unnecessary volatilization of the adsorbed molecules / ions.

[0063] In this embodiment, MoS 2 The materials are used as the first material 5 and the second material, and pure water is used as the precursor solution. The above steps are implemented, and then the control of the van der Waals gap is verified through testing.

[0064] For saturated steam at different temperatures, the adsorption amount on the surface of the first material 5 is different, and the size of the van der Waals gap formed is also different. Figure 4 A series of MoS with varying van der Waals gaps prepared by the present invention 2 Electron microscopy images of homogeneous structures (scale is 5 nm), which show the measurement results of the formation of van der Waals gaps in an environment without steam and in an environment with saturated steam at different temperatures (40℃-100℃), such as Figure 4 As shown, MoS 2 The size of the van der Waals gap of the homogap structure can vary between 0.55-5.36 nm.

[0065] Figure 5 A series of van der Waals gap structures of different types and dimensions prepared by the present invention (including elemental analysis), which shows the curve diagram of the van der Waals gap size formed under saturated steam at different temperatures, according to Figure 5 It can be seen that the gap can reach its maximum at about 100°C, and the gap size no longer increases significantly as the temperature increases further.

[0066] Embodiment 2

[0067] The method for controlling the van der Waals gap provided by the present invention is applicable to 2D and / or 3D materials and has universal applicability.

[0068] Embodiment 2 of the present invention provides a series of van der Waals gap structures of different types and dimensions prepared by using different materials as the first material and the second material, so as to illustrate the universality of the method for controlling the van der Waals gap provided by the present invention.

[0069] like Figure 6 As shown, the present invention uses Graphene and Graphene, MoTe 2 and MoTe 2 、PdSe 2 and PdSe 2 Prepare homojunction using WS 2 and MoS 2 、ReS 2 and MoS 2 、Semiconductor-PtS 2 and semiconductor-MoS2 , p-type-WSe 2 and n-type-MoS 2 、Semiconductor PdSe 2 and semiconductor MoS 2 Fabrication of heterojunctions using 3D Au films and semiconductor MoS 2 , 3D Au films and P + Si is used to prepare metal / semiconductor junctions, pure water is used as the precursor solution, and the method for controlling the van der Waals gap as described in Example 1 is used under saturated steam conditions at 100°C to obtain the following Figure 6 The van der Waals gaps shown have values ​​of 5.27nm, 4.08nm, 6.46nm, 2.15nm, 3.14nm, 9.51nm, 2.91nm, 6.18nm, 2.39nm, and 4.77nm, respectively.

[0070] Experimental test results show that for different 2D and / or 3D material combinations, the sizes of the van der Waals gaps at an evaporation temperature of 100°C are different, which is caused by differences in defect states on the material surface and intrinsic hydrophilicity.

[0071] Experiments have shown that for different combinations of materials, the MoS 2 The material gap control scheme is used to regulate the van der Waals gap.

[0072] Embodiment 3

[0073] Embodiment 3 of the present invention provides a MoS prepared based on the method for controlling the van der Waals gap described in Embodiment 1. 2 / Gap superlattice conceptual structure.

[0074] Embodiment 3 of the present invention adopts the method provided by the present invention, and adopts four layers of MoS 2 The material stacking is as follows Figure 7 The gap structure shown. Figure 7 As shown, 1-MoS 2 Layer and 2-MoS 2 The gap I between the layers belongs to the intrinsic gap of the material, with a size of 0.18 nm. 2 Layer and 3-MoS 2 The gap II of the layer is 1.42nm, 3-MoS 2 Layer and 4-MoS 2 The interlayer gap III is 3.06 nm, which is obtained under the conditions of no steam, saturated steam at 40°C and 60°C, respectively.

[0075] Experiments have shown that the method for controlling the van der Waals gap provided by the present invention is also applicable to the preparation of gap superlattices.

[0076] Embodiment 4

[0077] Embodiment 4 of the present invention provides a MoS prepared based on the method for controlling the van der Waals gap described in Embodiment 1. 2 / iodide ion solution gap / MoS 2 Structure, the fourth embodiment of the present invention only replaces the pure water in the first embodiment with potassium iodide solution, Figure 8 The MoS prepared in this example 2 / iodide ion solution gap / MoS 2 Electron microscope images of the structure and the corresponding elemental spectra, such as Figure 8 As shown, when the evaporation temperature is set to 40 °C, the upper and lower MoS 2 There is a potassium iodide gap of uniform size in the middle of the layer, and the iodine element in the gap can be proved by the corresponding elemental spectrum.

[0078] Experiments show that in the method for controlling the van der Waals gap provided by the present invention, the precursor solution can be expanded to a solution containing different molecules / ions, etc.

[0079] In summary, the present invention provides a universal method for controlling the van der Waals gap, realizing the creation of the van der Waals gap, size regulation and gap component customization. The method provided by the present invention will have the potential to be applied to various aspects such as modulating material properties, customizing device performance, exploring extreme-size material science and realizing functional devices with new principles. At the same time, ultra-small van der Waals gaps are expected to achieve water filtration, ion screening, seawater desalination, etc.; large van der Waals gaps are expected to achieve pressure sensing, etc.

[0080] The protection scope of the present invention is not limited to the above-mentioned embodiments. Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the scope and spirit of the present invention. If these changes and modifications fall within the scope of the claims of the present invention and their equivalents, the present invention is intended to include these changes and modifications.

[0081] Many specific details are described in the above description to facilitate a full understanding of the present invention. However, the above description is only a preferred embodiment of the present invention. The present invention can be implemented in many other ways different from those described herein, so the present invention is not limited to the specific implementation disclosed above. At the same time, any person familiar with the art can make many possible changes and modifications to the technical solution of the present invention using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.

Claims

1. A method for controlling a van der Waals gap, characterized in that: The method comprises the following steps: Step 1, generating saturated steam using a precursor solution; Step 2, placing the first material in the saturated steam for molecular and / or ionic adsorption; Step 3, physically laminating the first material and the second material to form a van der Waals gap, wherein the size of the gap is controlled by the saturated steam in which the first material is adsorbed; The method is able to control the van der Waals gap of materials of different dimensions.

2. The method according to claim 1, characterized in that: The precursor solution is pure water or an aqueous solution containing different molecules / ions.

3. The method according to claim 1, characterized in that: The size of the gap is controlled by the temperature of the saturated steam in which the first material is adsorbed.

4. The method according to claim 1, characterized in that: In the step 2, the first material is a 2D and / or 3D material.

5. The method according to claim 1, characterized in that: The thickness of the first material is greater than 8 nm.

6. A MoS2 homojunction, characterized in that: The MoS2 homojunction is prepared according to the method according to any one of claims 1-5, and the first material and the second material are MoS2.

7. A MoS2 homojunction according to claim 6, characterized in that: The gap size of the MoS2 homojunction is 0.55nm-5.36nm.

8. A 2D / 3D heterojunction, characterized in that: The 2D / 3D heterojunction is prepared according to the method according to any one of claims 1 to 5, and the first material and the second material are 2D and / or 3D materials.

9. A multilayer MoS2 superlattice structure, characterized in that: The multilayer MoS2 superlattice structure is prepared according to the method according to any one of claims 1 to 5, the first material and the second material are MoS2, and the gap size of each layer of the multilayer MoS2 superlattice structure can be controlled.

10. A MoS2 / iodine ion solution gap / MoS2 structure, characterized in that: The MoS2 / iodine ion solution gap / MoS2 structure is prepared according to the method described in any one of claims 1-5, the first material and the second material are MoS2, and the precursor solution is an iodine ion solution.