A method for regenerating thallium poisoned catalyst
By real-time detection of the pH value rise rate and configuring a specific solution for ultrasonic cleaning and impregnation and calcination, the problem of inaccurate control of catalyst regeneration in thallium poisoning is solved, the removal of thallium and the recovery of catalyst activity are achieved, and the denitrification efficiency is improved.
Patent Information
- Application Number
- CN202410011099.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-04
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-01-04
AI Technical Summary
In the prior art, the regeneration control of thallium poisoning catalysts is inaccurate, resulting in long-term soaking in acidic solutions or high acidity affecting the catalyst structure and reducing denitrification efficiency.
Remove floating ash by blowing compressed air, remove residual ash and compounds by ultrasonic cleaning, configure peeling and regeneration solutions for cleaning, detect the pH value rise rate in real time to adjust the reaction time, use monoethanolamine and ammonium metavanadate for impregnation and calcination, forming Active substances to restore catalyst activity.
The accurate removal of thallium and the recovery of catalyst activity are achieved, the denitrification efficiency after regeneration is improved, the structural damage of the catalyst is avoided, and the long-term use of the catalyst is ensured.
Smart Images

Figure CN117899945B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of SCR denitration catalysts, and in particular to a regeneration method for a thallium poisoned catalyst. Background Art
[0002] Cement kiln flue gas contains a large amount of nitrogen oxides, and the country's requirements for atmospheric emissions are becoming increasingly stringent. More and more cement kilns use SCR denitrification catalysts to treat flue gas; cement kilns mainly use limestone, sandstone, fly ash, bauxite and pyrite as raw materials; and thallium (Tl) is a highly toxic dispersed element widely distributed in nature, and the Tl content in pyrite can reach 15.1 mg / kg; during the cement production process, Tl in the raw materials enters the flue gas through volatilization, causing thallium poisoning of the catalyst; after entering the catalyst, Tl first interacts with Ti-(OH)-Ti, and then forms a layer of thallium oxide covering layer on the catalyst surface; as the deposition amount of Tl continues to increase, thallium oxide completely covers the active component V, occupies and destroys the active site of the catalyst; at the same time, Tl, as a sulfur-philic element, reacts with SO2 in the flue gas to form Tl2SO4, which further covers the Tl2O3 layer on the catalyst surface; these Tl covering the catalyst surface cause the active site oxidation ability to be completely lost; this covering not only fails to improve the SCR reaction, but also increases N2O production, resulting in large-scale greenhouse gas emissions.
[0003] Thallium can cause catalyst deactivation, micropore clogging, and reduced specific surface area; the catalyst activity is low when slightly poisoned, and the catalyst is deactivated when severely poisoned; most other poisoning substances such as alkali metals and sulfur can be effectively removed by conventional regeneration technology, but there is currently little research on the regeneration of Tl poisoned catalysts; a crust will also form on the surface of the cement kiln thallium poisoned catalyst, which is covered with a large amount of ash, and thallium can also be detected in the ash; there is currently no special technology to treat these crusts; research on the regeneration of thallium poisoned catalysts can not only increase the service life of the catalyst, but also provide a basis for its resource utilization; the present invention is based on the form and properties of thallium on the catalyst, and invents a technical solution for effectively removing thallium from the catalyst and restoring the catalyst activity.
[0004] Chinese Patent Publication No.: CN111715210A discloses a regeneration method for a cement kiln thallium-poisoned SCR denitration catalyst. The technical point is that after the thallium-poisoned SCR denitration catalyst is dusted, cleaned, soaked, rinsed and dried, a titanium, vanadium and tungsten soluble active substance is implanted to cooperate with subsequent calcination to restore the catalyst activity. However, the concentration of sulfuric acid used in the regeneration method is relatively high, and there is a certain loss of active components of the catalyst. It can be seen that the existing regeneration method of the thallium-poisoned SCR denitration catalyst still cannot accurately judge the degree of thallium removal when realizing catalyst regeneration, resulting in the self-structure of the thallium-poisoned catalyst being affected in the acidic solution, thereby reducing the denitration efficiency of the regenerated catalyst. Summary of the invention
[0005] To this end, the present invention provides a regeneration method for a thallium poisoned catalyst, so as to overcome the problem that the regeneration control of the thallium poisoned catalyst in the prior art is inaccurate, resulting in the thallium poisoned catalyst being immersed in an acidic solution for a long time or in an acidic solution with a high acid concentration, which affects the catalyst structure and reduces the denitrification efficiency of the regenerated catalyst.
[0006] To achieve the above object, the present invention provides a method for regenerating a thallium poisoned catalyst, comprising:
[0007] Step S1, removing floating dust on the surface of the thallium poisoned catalyst by compressed air blowing or negative pressure cleaning;
[0008] Step S2, washing the thallium poisoned catalyst with deionized water under ultrasonic bubbling conditions to remove residual ash and water-soluble compounds on the surface of the thallium poisoned catalyst;
[0009] Step S3, preparing a peeling solution, immersing the thallium poisoned catalyst in the peeling solution, and cleaning it under ultrasonic bubbling conditions;
[0010] Step S4, soaking the thallium poisoned catalyst in deionized water, and washing it under ultrasonic bubbling conditions to remove the peeling solution remaining on the thallium poisoned catalyst;
[0011] Step S5, preparing a regeneration solution, using the regeneration solution to clean the thallium poisoned catalyst by ultrasonic bubbling at room temperature, and performing real-time detection on the pH value of the regeneration solution, calculating the real-time rising rate of the real-time pH value of the regeneration solution, and determining whether to adjust the preset reaction time or determine that the regeneration reaction is completed;
[0012] Step S6, soaking the thallium poisoned catalyst in deionized water and cleaning it under ultrasonic bubbling conditions;
[0013] Step S7, using monoethanolamine and ammonium metavanadate to prepare a metavanadate solution, impregnating the thallium poisoned catalyst and drying it;
[0014] Step S8, calcining the precursor impregnated on the thallium poisoned catalyst to form a corresponding active substance, thereby completing the regeneration of the thallium poisoned catalyst.
[0015] Furthermore, in step S3, the peeling solution is configured as a mixed solution of an acid and a dispersant, wherein the acid includes but is not limited to one or more of sulfuric acid, hydrochloric acid, and nitric acid, and the dispersant includes but is not limited to one or more of sodium dodecyl sulfate, Tween 20, polyethylene glycol 1000, polyoxyethylene lauryl ether, polyethylene glycol, Tween 80, and sodium isooctyl sulfosuccinate.
[0016] Furthermore, in step S5, the real-time pH value of the configured regeneration solution is detected, and the real-time rising rate of the real-time pH value of the regeneration solution is calculated, the real-time rising rate difference is calculated according to the real-time rising rate and the standard rising rate, and when the real-time rising rate difference is less than or equal to the standard rising rate difference, the regeneration reaction of the thallium poisoned catalyst is controlled with a preset reaction time.
[0017] Furthermore, in step S5, if the calculated real-time rising rate difference of the real-time pH value of the regeneration solution is greater than the standard rising rate difference, the real-time rising rate is compared with the standard rising rate to determine the reaction state of the thallium poisoning catalyst in the regeneration solution.
[0018] Further, in step S5, if the calculated real-time rising rate difference of the real-time pH value of the regeneration solution is greater than the standard rising rate difference, and the real-time rising rate is greater than the standard rising rate, the preset reaction time is reduced according to the real-time rising rate and the standard rising rate, and the regeneration reaction of the thallium poisoning catalyst is controlled with the adjusted preset reaction time;
[0019] Among them, Tm′=Tm-Tm×[(Vs-Vb) / Vs], Tm is the preset reaction time, Tm′ is the preset reaction time after adjustment, Vs is the real-time rising rate of the real-time pH value of the regeneration solution, and Vb is the standard rising rate of the pH value.
[0020] Furthermore, in step S5, if the calculated real-time rising rate difference of the real-time pH value of the regeneration solution is greater than the standard rising rate difference, and the real-time rising rate is less than the standard rising rate, the current reaction time of cleaning in the current regeneration solution is obtained, and based on the comparison result between the current reaction time and the set minimum reaction time, it is determined whether to increase the power of ultrasonic cleaning or make a regeneration termination judgment.
[0021] Furthermore, in step S5, a regeneration end rising rate is provided, and the regeneration end determination includes obtaining the pH value rising amount within the current detection time, calculating the unit rising rate according to the pH value rising amount within the current detection time, and comparing the unit rising rate with the regeneration end rising rate.
[0022] If the unit rising rate is less than or equal to the rising rate at the end of regeneration, the reaction is judged to have stopped and the regeneration solution cleaning is completed;
[0023] If the unit rising rate is greater than the regeneration end rising rate, the regeneration reaction of the thallium poisoned catalyst is controlled with a preset reaction time;
[0024] Among them, C z =C s -C s-1 , Vd=C z / t,C z The increase in pH value during the current detection time, C s To detect the real-time pH value of the regeneration solution, C s-1 The real-time pH value of the regeneration solution configured for the last detection time t is detected, t is the set detection time, and Vd is the unit rise rate corresponding to the calculated current detection time.
[0025] Furthermore, in the step S5, by setting the detection time, the real-time pH value of the configured regeneration solution is detected after each detection time, and the real-time rising rate of the real-time pH value of the regeneration solution is calculated;
[0026] Where Vs = (C s -C c ) / Ts,C s is the real-time pH value of the regeneration solution configured for detection, Vs is the real-time rising rate of the real-time pH value of the regeneration solution, C c is the initial pH value of the configured regeneration solution, and Ts is the current reaction time.
[0027] Furthermore, in step S5, the regeneration solution configured is one or a combination of an acid, a chelating agent, a dispersant, and an oxidant, wherein the acid includes but is not limited to sulfuric acid, hydrochloric acid, and nitric acid; the chelating agent includes but is not limited to oxalic acid, EDTA, EDTA·2Na, aminotrimethylenephosphonic acid, and glycolic acid; the oxidant includes but is not limited to H2O2, hypochlorous acid, etc.; the dispersant includes but is not limited to polyethylene glycol 600, Tween 80, sodium isooctyl sulfosuccinate, Tween 20, and polyethylene glycol 1000.
[0028] Furthermore, in step S7, ammonium metavanadate and monoethanolamine are added to deionized water in a mass ratio of 1:1, and stirred and mixed at 75°C±5°C to form a homogeneous solution, thereby completing the preparation of the metavanadate solution.
[0029] Compared with the prior art, the beneficial effects of the present invention are that, by real-time detection of the pH value of the regeneration solution, the real-time rising rate of the real-time pH value of the regeneration solution is calculated, and it is determined whether to adjust the preset reaction time or determine whether the regeneration reaction is completed, the real-time state of the reaction in the regeneration solution is accurately and efficiently detected, which is convenient for timely making corresponding adjustments and accurately determining whether the regeneration reaction is completed, thereby ensuring the accuracy of removing thallium and avoiding the situation where the regeneration solution is not completely cleaned; and by removing the dust and crust before the regeneration solution is cleaned, the thallium oxide layer is exposed, which is conducive to the full contact reaction between the reagent and the thallium during the subsequent chemical cleaning, thereby accelerating the reaction. Speed, improve reaction efficiency; when thallium is removed by regeneration solution, a certain amount of active substances will be lost in the cleaned catalyst. The active substances that have been impregnated and calcined are reloaded to ensure the removal of poisoning elements such as thallium, sulfur, calcium, sodium, etc. on the catalyst, and the activity of the catalyst is restored at the same time. The surface crust of the thallium-poisoned catalyst is removed by peeling solution to improve the regeneration efficiency of the catalyst. The regeneration solution is configured and the catalyst is regenerated under pH monitoring to achieve the purpose of removing poisoning elements and restoring activity. At the same time, the reaction time of the catalyst in the regeneration solution is accurately controlled to improve the denitrification efficiency of the regenerated catalyst.
[0030] Furthermore, the alkaline oxide is dissolved by acid, and the chelating agent is used to combine with thallium to form a complex to clean the thallium on the catalyst. In an acidic environment, some alkali metals that are insoluble in water can also be removed, and the chelating agent can also combine with calcium on the catalyst to increase the calcium removal rate. At the same time, adding dispersants and oxidants can enhance the removal efficiency of thallium, increase the cleaning effect of micropores, improve the removal efficiency and specific surface area, and facilitate the regeneration of thallium-poisoned catalysts.
[0031] Furthermore, by setting the standard rising rate and the standard rising rate difference to form a standard rising rate range, when the rising rate of the pH value exceeds the standard range, it is judged whether the real-time rising rate of the pH value Vs exceeds the standard rising rate of the pH value, which is helpful to clarify whether the current regeneration reaction is fast or slow, and facilitate the next adjustment and improvement.
[0032] In particular, by shortening the preset reaction time when the real-time rising rate of the pH value is greater than the standard rising rate of the pH value, it is helpful to reduce unnecessary regeneration reaction time, reduce the impact of the regeneration solution on the catalyst structure, improve the regeneration reaction efficiency, and enhance the regeneration effect of the catalyst.
[0033] Furthermore, by calculating the pH value increase C during the current detection time z The unit rising rate is used to determine whether the regeneration reaction has stopped, so as to avoid the adverse effects of the regeneration solution on other substances of the catalyst after the regeneration reaction is completed, thereby ensuring the accuracy of the regeneration of the thallium poisoned catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a flow chart of a regeneration method for a thallium-poisoned catalyst according to an embodiment of the present invention;
[0035] Figure 2 This is a comparison chart of the NOx removal performance of various samples in the embodiments of the present invention;
[0036] Figure 3 The diagram shows the crust removal effects of different embodiments of the present invention. DETAILED DESCRIPTION
[0037] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0039] It should be noted that, in the description of the present invention, terms such as "up", "down", "left", "right", "inside" and "outside" indicating directions or positional relationships are based on the directions or positional relationships shown in the drawings. This is merely for the convenience of description and does not indicate or imply that the device or element must have a specific orientation, be constructed and operated in a specific orientation. Therefore, it cannot be understood as a limitation on the present invention.
[0040] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0041] See also Figure 1 As shown, it is a flow chart of a regeneration method for a thallium-poisoned catalyst according to an embodiment of the present invention. This embodiment provides a regeneration method for a thallium-poisoned catalyst, comprising:
[0042] Step S1, removing floating dust on the surface of the thallium poisoned catalyst by compressed air blowing or negative pressure cleaning;
[0043] Step S2, washing the thallium-poisoned catalyst treated in step S1 with deionized water under ultrasonic bubbling conditions to remove the residual ash on the catalyst surface and wash off the water-soluble compounds, wherein Tl2SO4 is also a water-soluble compound, so water washing can also remove part of Tl;
[0044] Step S3, preparing a peeling solution, immersing the thallium-poisoned catalyst treated in step S2 in the peeling solution, and cleaning it under ultrasonic bubbling conditions;
[0045] Step S4, soaking the thallium-poisoned catalyst treated in step S3 in deionized water, and washing it under ultrasonic bubbling conditions to remove the peeling solution remaining on the thallium-poisoned catalyst to prevent affecting the subsequent thallium removal step;
[0046] Step S5, preparing a regeneration solution, using the regeneration solution to ultrasonically clean the thallium-poisoned catalyst treated in step S4 at room temperature, and performing real-time detection of the pH value of the regeneration solution, calculating the real-time rising rate of the real-time pH value of the regeneration solution, and determining whether to adjust the preset reaction time or determine that the regeneration reaction is completed;
[0047] Step S6, soaking the thallium-poisoned catalyst treated in step S5 in deionized water, and cleaning it under ultrasonic bubbling conditions to clean the residual regeneration solution and thallium on the thallium-poisoned catalyst to avoid affecting the subsequent impregnation steps;
[0048] Step S7, using monoethanolamine and ammonium metavanadate to prepare a metavanadate solution, impregnating the thallium poisoned catalyst treated in step S6, and drying at 60° C. for 24 hours;
[0049] Step S8, calcining the precursor impregnated on the thallium poisoned catalyst in step S7 into a corresponding active material at 300° C. for 3 hours.
[0050] The surface of the thallium (Tl) poisoned catalyst contains a lot of ash and there is a crust on the surface. Therefore, ash removal is required before regeneration and cleaning. The floating ash on the surface can be removed by physical cleaning means. The crust needs to be configured with a specific peeling solution. Thallium removal requires a regeneration solution. The catalyst after cleaning will lose a certain amount of active substances. The active substances are reloaded by impregnating and calcining the active substances to ensure the removal of poisoning elements such as thallium, sulfur, calcium, and sodium on the catalyst. At the same time, the activity of the catalyst is restored. The surface crust of the thallium poisoned catalyst is removed by the peeling solution to improve the catalyst regeneration efficiency. The catalyst is regenerated under specific conditions and processes by configuring the regeneration solution to achieve the purpose of removing poisoning elements and restoring activity.
[0051] The regeneration solution includes acid, chelating agent, dispersant and oxidant. Thallium oxide is an alkaline oxide. Acid is used to dissolve it, and a chelating agent is used to combine with thallium to form a complex to clean the thallium on the catalyst. In an acidic environment, some alkali metals that are insoluble in water can also be removed, and the chelating agent can also combine with calcium on the catalyst to increase the calcium removal rate; adding dispersants and oxidants at the same time can enhance the removal efficiency of thallium, increase the cleaning effect of micropores, and improve the removal efficiency and specific surface area.
[0052] The main components of the crust are calcium carbonate, calcium sulfate and iron oxide. The crust is removed by configuring a specific peeling solution to expose the thallium oxide layer, which is conducive to the full contact and reaction between the reagent and thallium during the subsequent chemical cleaning, accelerating the reaction speed and improving the reaction efficiency. The specific solution includes one or a combination of acid, dispersant, and non-ionic surfactant. The acidic solution can remove calcium carbonate and loosen the crust. Bubbling and ultrasound can increase the fluidity of water, create certain hydraulic conditions, and wash off the loose crust. By adding dispersants or non-ionic surfactants to change the surface properties of the catalyst and ash, the micropores inside the catalyst are cleaned to increase the specific surface area.
[0053] Specifically, in step S3, the peeling solution is prepared as a mixed solution of an acid and a dispersant, the acid source includes but is not limited to sulfuric acid, hydrochloric acid, and nitric acid, and the dispersant includes but is not limited to sodium dodecyl sulfate (SDS), Tween 20 (Tween-20), polyethylene glycol 1000 (PEG-1000), polyoxyethylene lauryl ether (PGME), polyethylene glycol 600 (PEG-600), Tween 80 (Tween-80), and sodium isooctyl sulfosuccinate.
[0054] Specifically, in step S5, a detection time t is set, and the real-time pH value C of the configured regeneration solution is detected every detection time t. s , calculate the pH rise C z , C z =C s -C s-1 , and calculate the real-time rising rate Vs of the real-time pH value of the regeneration solution, Vs = (C s -C c ) / Ts;
[0055] Among them, C z is the increase in pH value, C s To detect the real-time pH value of the regeneration solution, C s-1 is the real-time pH value of the regeneration solution configured for the last detection time t, Vs is the real-time rising rate of the real-time pH value of the regeneration solution, C c is the initial pH value of the configured regeneration solution, Ts is the current reaction time;
[0056] Specifically, in step S5, a standard rising rate range is further provided, including a standard rising rate Vb and a standard rising rate difference ΔVb. After detecting the real-time pH value of the configured regeneration solution, the real-time rising rate Vs of the real-time pH value of the regeneration solution is calculated, and the real-time rising rate difference ΔVs is calculated according to the real-time rising rate Vs and the standard rising rate Vb, ΔVs=|Vb-Vs|, and the standard rising rate difference ΔVb is compared with the real-time rising rate difference ΔVs for determination.
[0057] When ΔVs≤ΔVb, it is determined that the real-time rising rate difference of the pH value is less than or equal to the standard rising rate difference, indicating that the rising rate of the pH value is within the standard range so far, and the regeneration reaction process is not adjusted;
[0058] When ΔVs>ΔVb, it is determined that the real-time rising rate difference of the pH value is greater than the standard rising rate difference, indicating that the rising rate of the pH value has exceeded the standard range so far. The real-time rising rate Vs is then compared with the standard rising rate Vb to determine the reaction state of the thallium poisoning catalyst in the regeneration solution.
[0059] By setting the standard rising rate and the standard rising rate difference to form a standard rising rate range, when the rising rate of the pH value exceeds the standard range, it is judged whether the real-time rising rate of the pH value Vs exceeds the standard rising rate of the pH value, which is helpful to clarify the speed and sufficiency of the current regeneration reaction and facilitate the next adjustment and improvement.
[0060] Specifically, in step S5, a preset reaction time Tm is set, and when the real-time pH value rising rate difference is greater than the standard pH value rising rate difference, the real-time pH value rising rate Vs is compared with the standard pH value rising rate Vb.
[0061] When Vs<Vb, it is determined that the real-time rising rate of the pH value is less than the standard rising rate of the pH value, and the current reaction time is determined to determine whether to increase the power of the ultrasonic bubbling cleaning;
[0062] When Vs>Vb, it is determined that the real-time rising rate of the pH value is greater than the standard rising rate of the pH value, and the preset reaction time is adjusted to Tm′, and when the real-time reaction time reaches the preset reaction time, the regeneration solution cleaning is completed;
[0063] Wherein, Tm′=Tm-Tm×[(Vs-Vb) / Vs], Tm is the preset reaction time, Vs is the real-time rising rate of the pH value, and Vb is the standard rising rate of the pH value.
[0064] In this embodiment, the pH value of the configured regeneration solution is usually 1.3, the set standard rising rate corresponds to 0.017 / minute, the set standard rising rate difference is 0.005 / minute, and the set detection time directly affects the accuracy of reaction control. At the same time, it must also be set accordingly with the detection speed and detection accuracy of the pH detection equipment. In this embodiment, a three-level pH electronic measuring instrument is used, and the detection time is set to 30 seconds, i.e. 0.5 minutes. In actual detection, it can be set accordingly according to the detection method or the type of instrument, generally not exceeding 3 minutes.
[0065] By shortening the preset reaction time when the real-time rising rate of the pH value is greater than the standard rising rate of the pH value, it is helpful to reduce unnecessary regeneration reaction time and improve the regeneration reaction efficiency.
[0066] In this embodiment, the preset reaction time is affected by factors such as the concentration of acidic substances in the regeneration solution, the concentration of chelating agent substances, the concentration of dispersant substances, and the concentration of oxidant substances, and should be set specifically based on actual conditions. In this embodiment, the preset reaction time is set to 30 minutes, and the corresponding minimum reaction time is 16 minutes. The specific setting value needs to be adjusted based on actual conditions and the actual concentration of substances in the regeneration solution, and will not be elaborated here.
[0067] Specifically, in step S5, the minimum reaction time Tb is set, and when the real-time rising rate difference of the pH value is greater than the standard rising rate difference, and the real-time rising rate of the pH value is less than the standard rising rate of the pH value, the current reaction time Ts is obtained, and the current reaction time Ts is compared with the minimum reaction time Tb.
[0068] When Ts ≥ Tb, the current reaction time is determined to be greater than or equal to the minimum reaction time, indicating that the current reaction time exceeds the minimum reaction time, and the pH value increase C within the current detection time is calculated. z The unit rising rate is determined and judged to determine whether to stop cleaning;
[0069] When Ts<Tb, it is determined that the current reaction time is less than the minimum reaction time, indicating that the current reaction time has not reached the minimum reaction time, and the catalyst regeneration is in the initial stage and has not yet fully participated in the reaction. Therefore, the power of ultrasonic cleaning needs to be increased. The increase is usually 20% to 60% of the initial cleaning power until the real-time rising rate Vs of the real-time pH value of the regeneration solution reaches or exceeds the standard rising rate range, or the current reaction time Ts reaches the minimum reaction time, and the power of ultrasonic cleaning is adjusted to the initial cleaning power.
[0070] By comparing the current reaction time Ts with the minimum reaction time Tb, it is determined which stage the current reaction is in. If the current reaction time is less than the minimum reaction time, the power of ultrasonic cleaning is increased to ensure that the reaction can start as soon as possible, improve the reaction efficiency, and ensure that the regeneration reaction can proceed normally.
[0071] Specifically, in step S5, a regeneration end rising rate Vz is set. When the real-time rising rate difference of the pH value is greater than the standard rising rate difference, the real-time rising rate of the pH value is less than the standard rising rate of the pH value, and the current reaction time is greater than or equal to the minimum reaction time, the pH value rise amount C within the current detection time is calculated. z The unit rate of increase Vd, Vd = C z / t, compare the unit rise rate Vd with the regeneration end rise rate Vz,
[0072] When Vd≤Vz, determine the pH value rise C within the current detection time. z The unit rising rate is less than the rising rate at the end of regeneration, indicating that the regeneration reaction stops and the regeneration solution cleaning is completed;
[0073] When Vd>Vz, determine the pH value increase C within the current detection time. z If the unit rising rate is greater than the rising rate at the end of regeneration, the regeneration solution is allowed to continue reacting until the current reaction time Ts reaches the preset reaction time Tm, the regeneration reaction is stopped, and the regeneration solution cleaning is completed.
[0074] By calculating the pH value increase C during the current detection time z The unit rising rate is used to determine whether the regeneration reaction has stopped, so as to avoid the adverse effects of the regeneration solution on other substances of the catalyst after the regeneration reaction is completed, thereby ensuring the accuracy of the regeneration of the thallium poisoned catalyst.
[0075] In this embodiment, the regeneration end rising rate Vz is set to 0.004 / minute. When the unit rising rate within the current detection time is not higher than the regeneration end rising rate, it is determined that the reaction process in the regeneration solution is basically completed, and the regeneration cleaning operation is ended.
[0076] Specifically, in step S5, the regeneration solution configured is one or a combination of an acid, a chelating agent, a dispersant, and an oxidant; the acid includes but is not limited to sulfuric acid, hydrochloric acid, and nitric acid; the chelating agent includes but is not limited to oxalic acid, EDTA, EDTA·2Na, aminotrimethylenephosphonic acid (ATMP), and glycolic acid; the oxidizing agent includes but is not limited to H2O2, hypochlorous acid, etc.; the dispersant includes but is not limited to polyethylene glycol 600, Tween 80, sodium isooctyl sulfosuccinate, Tween 20 (Tween-20), and polyethylene glycol 1000 (PEG-1000).
[0077] Specifically, in step S7, an ammonium metavanadate solution is prepared: ammonium metavanadate (NH4VO3) and monoethanolamine (H2NCH2CH2OH) are added to deionized water in a mass ratio of 1:1, and stirred and mixed at 75°C±5°C to form a homogeneous solution.
[0078] Since ammonium metavanadate is insoluble in water, a certain amount of monoethanolamine needs to be added to dissolve it by heating. After being configured into a solution, it is beneficial to the dispersion of the active substance vanadium. Ammonium metavanadate is a precursor of the active ingredient V2O5, and it decomposes into V2O5 during calcination and is distributed in the catalyst.
[0079] Specifically, this embodiment 1 provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0080] Step S1, negative pressure cleaning: use -0.098MPa negative pressure cleaning to remove floating dust on the surface;
[0081] Step S2, water washing: washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0082] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with a mixed solution of 0.5% sulfuric acid and 1% polyethylene glycol under ultrasonic bubbling conditions for 30 minutes;
[0083] Step S4, water washing: the catalyst washed in step S3 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0084] Step S5, regeneration liquid cleaning: the catalyst cleaned with deionized water is cleaned with regeneration liquid by ultrasonic bubbling at room temperature for 30 minutes, and the regeneration liquid is configured as 5% sulfuric acid, 0.25% EDTA, and 1% polyethylene glycol 600;
[0085] Step S6, washing with deionized water for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0086] Step S7, immersing the dried catalyst in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0087] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0088] In addition, this embodiment 2 provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0089] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0090] Step S2, water washing: washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0091] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with a mixed solution of 0.5% nitric acid and 1% polyethylene glycol under ultrasonic bubbling conditions for 30 minutes;
[0092] Step S4, water washing: the catalyst washed in step S3 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0093] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling at room temperature for 30 minutes using a regeneration liquid, wherein the regeneration liquid is configured as 5% sulfuric acid and 3% oxalic acid;
[0094] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0095] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0096] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0097] Specifically, this embodiment 3 provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0098] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0099] Step S2, washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0100] Step S3, washing the catalyst treated in step S2 with 0.5% hydrochloric acid for 30 minutes under ultrasonic bubbling conditions;
[0101] Step S4, water washing: the catalyst washed in step S1 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0102] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling at room temperature for 30 minutes using a regeneration liquid, wherein the regeneration liquid is configured to be 5% sulfuric acid, 2% ATMP, Tween 80, and 0.5% H2O2;
[0103] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0104] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0105] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0106] Specifically, this embodiment 4 provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0107] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0108] Step S2, washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0109] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with a mixed solution of 0.5% sulfuric acid and 1% Tween 80 under ultrasonic bubbling conditions for 30 minutes;
[0110] The catalyst cleaned in step S4 and step S3 is cleaned with deionized water for 30 minutes to prevent interference with the next step;
[0111] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling at room temperature for 30 minutes using a regeneration liquid, wherein the regeneration liquid is configured as 5% sulfuric acid and 2% glycolic acid;
[0112] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0113] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0114] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0115] Specifically, this embodiment 5 provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0116] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0117] Step S2, water washing: washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0118] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with 0.5% hydrochloric acid for 30 minutes under ultrasonic bubbling conditions;
[0119] Step S4, water washing: the catalyst washed in step S3 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0120] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling at 80° C. for 30 min using a regeneration liquid, wherein the regeneration liquid is configured with 5% sulfuric acid and 0.02% EDTA;
[0121] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0122] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0123] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0124] Specifically, Comparative Example 1 of the present invention provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0125] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0126] Step S2, water washing: washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0127] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with 0.5% hydrochloric acid for 30 minutes under ultrasonic bubbling conditions;
[0128] Step S4, water washing: the catalyst washed in step S3 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0129] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling with regeneration liquid for 30 minutes, and the regeneration liquid is configured as 5% sulfuric acid;
[0130] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0131] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0132] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0133] Specifically, Comparative Example 2 of the present invention provides a method for regenerating a thallium poisoned catalyst, comprising the following steps:
[0134] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0135] Step S2, water washing: washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0136] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with 0.5% hydrochloric acid for 30 minutes under ultrasonic bubbling conditions;
[0137] Step S4, water washing: the catalyst washed in step S3 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0138] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling with regeneration liquid for 30 minutes, and the regeneration liquid is configured to be 2% ATMP;
[0139] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0140] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0141] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0142] Specifically, Comparative Example 3 of the present invention provides a regeneration method for a thallium poisoned catalyst, comprising the following steps:
[0143] Step S1, compressed air soot blowing: using compressed air to blow soot to remove floating dust on the surface;
[0144] Step S2, water washing: washing the catalyst treated in step S1 with deionized water for 30 minutes under ultrasonic bubbling conditions to remove water-soluble compounds and tiny particles attached to the catalyst;
[0145] Step S3, removing the crust: the catalyst treated in step S2 is cleaned with 0.5% hydrochloric acid for 30 minutes under ultrasonic bubbling conditions;
[0146] Step S4, water washing: the catalyst washed in step S3 is washed with deionized water for 30 minutes to prevent interference with the next step;
[0147] Step S5, regeneration liquid cleaning: the catalyst cleaned in step S4 is cleaned by ultrasonic bubbling with regeneration liquid for 30 minutes, and the regeneration liquid is configured with 2% polyethylene glycol;
[0148] Step S6, washing: using deionized water to wash for 30 minutes to remove the residual compounds on the catalyst in step S5, and drying at 60° C. for 8 hours;
[0149] Step S7, activation: immerse the catalyst of step S6 in a metavanadium solution for 10 minutes, wherein the ratio of ammonium metavanadate and monoethanolamine added to the metavanadium solution is 1:1, and the concentration of ammonium metavanadate in the final solution is 5%.
[0150] Step S8, calcination: calcine the catalyst prepared in step S7 at 400° C. for 3 h.
[0151] Specifically, the finished catalyst was evaluated and tested in terms of specific surface area, denitration performance, and catalyst chemical composition according to the national standard GBT 31587-2015 honeycomb flue gas denitration catalyst. The microscopic specific surface area was calculated using the BET method, and the detection instrument was the BSD-PS2 specific surface and pore size analyzer manufactured by Best Instrument Technology (Beijing) Co., Ltd. The chemical composition of the sample was analyzed using an X-ray fluorescence spectrometer, and the detection instrument was the PW4400 / 10 X-ray fluorescence spectrometer produced by PANalytical in the Netherlands. The microscopic specific surface area and chemical composition of the sample are shown in Table 1.
[0152]
[0153] Table 1 Composition and microscopic specific surface area test results
[0154] The spent catalyst was cut into rectangular test samples of the same size, with 2×2 holes and a length of 40 cm. The samples were regenerated in an ultrasonic device according to the above-mentioned steps of the example and the comparative example. The regenerated catalyst was loaded into a reactor for denitration test. The test conditions were as follows: the reaction system temperature was 290°C, the mixed gas space velocity was 5000h -1, mixed gas content: NOx194ppm, O210%, N2 as carrier gas. The gases from each route are mixed by mass flow meter and heated by mixing preheater before entering the reactor; the gas is collected at the inlet and outlet sampling ports with testo350-EPA portable flue gas analyzer for analysis. The NOx removal performance of each sample is as follows Figure 2 shown.
[0155] According to Table 1 and Figure 2 It can be seen that the present invention has a good regeneration effect on thallium-poisoned waste catalysts, and the thallium removal rate after regeneration reaches 94%, and other poisoning components such as sulfur and calcium are also removed. The original component tungsten is not lost, and vanadium is basically restored after activation and impregnation with a low-concentration metavanadium solution. After regeneration and calcination, the denitrification efficiency can reach more than 90%.
[0156] The present invention lists 5 embodiments and 3 comparative examples, including 4 different methods for removing crusts. Figure 3 As shown, it can be seen that the skin on the surface of the catalyst in Example 3 is basically removed, no residual skin is left, and the specific surface area is restored to a higher degree.
[0157] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
[0158] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for regenerating a thallium-poisoned catalyst, characterized in that: include, Step S1, removing floating dust on the surface of the thallium poisoned catalyst by compressed air blowing or negative pressure cleaning; Step S2, washing the thallium poisoned catalyst with deionized water under ultrasonic bubbling conditions to remove residual ash and water-soluble compounds on the surface of the thallium poisoned catalyst; Step S3, preparing a peeling solution, immersing the thallium poisoned catalyst in the peeling solution, and cleaning it under ultrasonic bubbling conditions; Step S4, soaking the thallium poisoned catalyst in deionized water, and washing it under ultrasonic bubbling conditions to remove the peeling solution remaining on the thallium poisoned catalyst; Step S5, preparing a regeneration solution, using the regeneration solution to clean the thallium poisoned catalyst by ultrasonic bubbling at room temperature, and performing real-time detection on the pH value of the regeneration solution, calculating the real-time rising rate of the real-time pH value of the regeneration solution, and determining whether to adjust the preset reaction time or determine that the regeneration reaction is completed; Step S6, soaking the thallium poisoned catalyst in deionized water and cleaning it under ultrasonic bubbling conditions; Step S7, using monoethanolamine and ammonium metavanadate to prepare a metavanadate solution, impregnating the thallium poisoned catalyst and drying it; Step S8, calcining the precursor impregnated on the thallium poisoned catalyst to form a corresponding active substance, thereby completing the regeneration of the thallium poisoned catalyst; In the step S5, the real-time pH value of the configured regeneration solution is detected, and the real-time rising rate of the real-time pH value of the regeneration solution is calculated, and the real-time rising rate difference is calculated according to the real-time rising rate and the standard rising rate, and when the real-time rising rate difference is less than or equal to the standard rising rate difference, the regeneration reaction of the thallium poisoning catalyst is controlled with a preset reaction time; In the step S5, if the calculated real-time rising rate difference of the real-time pH value of the regeneration solution is greater than the standard rising rate difference, the real-time rising rate is compared with the standard rising rate to determine the reaction state of the thallium poisoning catalyst in the regeneration solution; In the step S5, if the calculated real-time rising rate difference of the real-time pH value of the regeneration solution is greater than the standard rising rate difference, and the real-time rising rate is greater than the standard rising rate, the preset reaction time is reduced according to the real-time rising rate and the standard rising rate, and the regeneration reaction of the thallium poisoning catalyst is controlled with the adjusted preset reaction time; Wherein, Tm′=Tm-Tm×[(Vs-Vb) / Vs], Tm is the preset reaction time, Tm′ is the preset reaction time after adjustment, Vs is the real-time rising rate of the real-time pH value of the regeneration solution, and Vb is the standard rising rate of the pH value; In step S5, if the calculated real-time rising rate difference of the real-time pH value of the regeneration solution is greater than the standard rising rate difference, and the real-time rising rate is less than the standard rising rate, the current reaction time of cleaning in the current regeneration solution is obtained, and according to the comparison result between the current reaction time and the set minimum reaction time, it is determined whether to increase the power of ultrasonic cleaning or perform the regeneration end judgment; In step S5, a regeneration end rising rate is provided, and the regeneration end determination includes obtaining the pH value rise amount within the current detection time, calculating the unit rising rate according to the pH value rise amount within the current detection time, and comparing the unit rising rate with the regeneration end rising rate. If the unit rising rate is less than or equal to the rising rate at the end of regeneration, the reaction is determined to be stopped and the regeneration solution cleaning is completed; if the unit rising rate is greater than the rising rate at the end of regeneration, the regeneration reaction of the thallium poisoned catalyst is controlled with a preset reaction time; Wherein, Cz=Cs-Cs-1, Vd=Cz / t, Cz is the pH value rise within the current detection time, Cs is the real-time pH value of the regeneration solution configured for detection, Cs-1 is the real-time pH value of the regeneration solution configured for the previous detection time t, t is the set detection time, and Vd is the calculated unit rise rate corresponding to the current detection time; In the step S5, by setting the detection time, the real-time pH value of the configured regeneration solution is detected after each detection time, and the real-time rising rate of the real-time pH value of the regeneration solution is calculated; Wherein, Vs = (Cs-Cc) / Ts, Cs is the real-time pH value of the regeneration solution configured for detection, Vs is the real-time rising rate of the real-time pH value of the regeneration solution, Cc is the initial pH value of the configured regeneration solution, and Ts is the current reaction time; In the step S7, ammonium metavanadate and monoethanolamine are added to deionized water in a mass ratio of 1:1, and stirred and mixed at 75° C.±5° C. to form a homogeneous solution, thereby completing the preparation of the metavanadate solution.
2. The regeneration method for a thallium poisoned catalyst according to claim 1, characterized in that: In step S3, the peeling solution is configured as a mixed solution of an acid and a dispersant, wherein the acid includes but is not limited to one or more of sulfuric acid, hydrochloric acid, and nitric acid, and the dispersant includes but is not limited to one or more of sodium dodecyl sulfate, Tween 20, polyethylene glycol 1000, polyoxyethylene lauryl ether, polyethylene glycol, Tween 80, and sodium isooctyl sulfosuccinate.
3. The regeneration method for a thallium poisoned catalyst according to claim 1, characterized in that: In step S5, the regeneration solution is configured to be one or a combination of an acid, a chelating agent, a dispersant, and an oxidant, wherein the acid includes but is not limited to sulfuric acid, hydrochloric acid, and nitric acid; the chelating agent includes but is not limited to oxalic acid, EDTA, EDTA·2Na, aminotrimethylenephosphonic acid, and glycolic acid; the oxidant includes but is not limited to H2O2, hypochlorous acid, etc.; the dispersant includes but is not limited to polyethylene glycol 600, Tween 80, sodium isooctyl sulfosuccinate, Tween 20, and polyethylene glycol 1000.