Decorative paper with low ink consumption and preparation method thereof

Through the combination of modified emulsion and polypropylene, a core-shell structure is formed, which solves the problems of water resistance and insufficient ink adhesion of decorative paper, and achieves more efficient ink use and better decorative paper performance.

CN117926642BActive Publication Date: 2024-12-06ZHE JIANG JIN SHANG TIAN CAI XIN CAI LIAO YOU XIAN GONG SI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410241704.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-04
Publication Date
2024-12-06
Estimated Expiration
2044-03-04

AI Technical Summary

Technical Problem

Existing decorative papers have shortcomings in water resistance and ink adhesion, resulting in excessive ink consumption and prone to deinking problems.

Method used

The modified emulsion is prepared from shell monomer, core monomer, modifier, initiator, emulsifier and buffer. The core-shell structure is formed by emulsion polymerization, combined with polypropylene material to improve the adhesion and water resistance of ink.

Benefits of technology

It significantly improves the ink adhesion and water resistance of decorative paper, reduces ink consumption, and enhances the mechanical properties of decorative paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004724589290000091
    Figure BDA0004724589290000091
  • Figure BDA0004724589290000092
    Figure BDA0004724589290000092
  • Figure BDA0004724589290000101
    Figure BDA0004724589290000101
Patent Text Reader

Abstract

The invention discloses a decorative paper with low ink consumption and a preparation method thereof. The decorative paper comprises a modified emulsion and polypropylene. The modified emulsion is prepared from a shell monomer, a core monomer, a modifier, an initiator, an emulsifier, and a buffer. First, the organic silicon monomer in the modifier is cross-linked with the core monomer, and then the core monomer and the shell monomer are free radical polymerized under the action of the initiator, the emulsifier, and the buffer, thereby obtaining the modified emulsion; finally, the modified emulsion is mixed with a polypropylene material and the decorative paper is prepared by a coating technology. Compared with the prior art, the decorative paper prepared by the invention has the advantages of strong water resistance, strong ink adhesion, and reduced ink consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of decorative paper, and in particular to a decorative paper with low ink consumption and a preparation method thereof. Background Art

[0002] The development of the decorative paper industry can be traced back to the 1980s. At that time, with the rapid development of my country's construction industry, people's demand for interior decoration continued to grow. Decorative paper, as an important interior decoration material, gradually attracted the attention of the market. Decorative paper is a special paper that is made by printing decorative base paper, impregnating it with resin and drying it to make a film paper. It is pressed on the surface of the board under high temperature conditions to decorate and protect the artificial board. At present, the printing of decorative paper is mainly gravure printing. This printing method has the advantages of large ink volume, high overprint accuracy, and simple quality control, but it has the disadvantages of long pre-press roller production cycle, complex technology, and high unit cost for small batch printing. With the development of society and the improvement of people's living standards, more and more people have begun to favor personalized, diversified and customized decoration and hope to print family photos, personal design works, corporate logos, and some novel and unique and meaningful pictures and texts on the surface of furniture. Obviously, gravure printing is difficult to meet this new demand.

[0003] Inkjet printing is a non-contact printing method developed in the 1970s. It uses electrical signals to control the high-speed flow of extremely small liquid ink droplets or extremely fine solid ink particles to generate images on the surface of the recording medium. It has the advantages of a wide range of substrates, flexible printing format, thick ink layer, strong adhesion, wide color gamut, bright colors, and high image and text quality.

[0004] CN116289332A discloses a hydrophobic and dirt-resistant decorative paper and a production method thereof, comprising a decorative base paper, wherein an ink layer and a glue layer are sequentially formed on the surface of the decorative base paper, wherein the glue layer is obtained by treating with a hydrophobic impregnating glue, wherein the hydrophobic impregnating glue comprises: an aqueous acrylic emulsion, a hyperbranched organosilicon polymer, a nanofiller, a silane coupling agent, a crosslinking agent, and water; and the hyperbranched organosilicon polymer comprises: a double-terminal hydrogenated silicone oil, glycidyl methacrylate, a chloroplatinic acid catalyst, dipropylenetriamine, and isopropanol. Although the decorative paper prepared by the method improves the hydrophobic effect of the decorative paper and is formaldehyde-free, the decorative paper prepared by the method has a multi-layer structure, and the connection performance between the layers is not very tight, and the decorative paper is prone to cracking.

[0005] CN103276631B discloses an environmentally friendly bathroom composite decorative paper and a manufacturing method thereof, comprising titanium powder paper as a substrate; the upper surface of the titanium powder paper is sequentially covered with a wear-resistant medium spray layer, a printing ink layer, a melamine spray layer and an acrylic spray layer; and the following steps are performed: 1) modifying the titanium powder paper; 2) printing ink 2-6 times on the wear-resistant medium spray layer to form a printing ink layer; 3) spraying melamine glue on the printing ink layer, and then drying to form a melamine spray layer; 4) spraying a water-based acrylic emulsion on the melamine spray layer, and then drying at a temperature of 160-180°C to form an acrylic coating layer. The decorative paper prepared by the method has the characteristics of excellent water resistance, can be rolled and placed, and is suitable for outdoor use. However, due to the different layer structures involved, the connectivity between the different layer structures is not strong, and de-inking is easily caused after the ink is sprayed.

[0006] Ordinary decorative base paper for printing is made of high-quality wood pulp and titanium dioxide as the main raw materials. When directly performing color inkjet printing, the ink quickly penetrates into the paper, resulting in low color density and poor resolution of the pattern. Especially when using polypropylene synthetic paper to make decorative paintings, since decorative paintings have the characteristics of bright colors, rich textures, and not easy to deform, the printing quality requirements of decorative paper cannot be met in terms of color and clarity, or various problems such as excessive consumption of ink occur. Summary of the invention

[0007] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to improve the water resistance and ink adhesion of the decorative paper, thereby reducing the ink consumption problem.

[0008] To achieve the above object, the present invention provides a low ink consumption decorative paper, which comprises, by weight: a modified emulsion and polypropylene, wherein the modified emulsion is prepared from a shell monomer, a core monomer, a modifier, an initiator, an emulsifier and a buffer.

[0009] The preparation method of the modified emulsion comprises the following steps:

[0010] S1. Add emulsifier, initiator, buffer and water into a reaction kettle, stir, raise the temperature to 75-90°C, add nuclear monomer dropwise within 10-20 minutes, keep warm for 10-40 minutes, and obtain seed emulsion;

[0011] S2, dropwise adding core monomer, emulsifier, initiator and water into the seed emulsion of S1 for 1-3 hours, and keeping the temperature at 75-90°C for 10-50 minutes after dropwise addition to obtain core layer emulsion;

[0012] S3, add shell monomer, modifier, initiator and water to the S2 core layer emulsion dropwise for 2-5 hours, keep warm at 75-90°C for 1-2 hours, and obtain a core-shell emulsion;

[0013] S4. Cool the S3 core-shell emulsion to 25-38°C, adjust the pH to 8-9 with aqueous ammonia, and filter out the precipitate to obtain a modified emulsion.

[0014] Preferably, the preparation method of the modified emulsion comprises the following steps, measured in parts by weight:

[0015] S1. Add 1-10 parts of emulsifier, 1-8 parts of initiator, 2-9 parts of buffer, and 20-40 parts of water into a reaction kettle, stir, and heat to 75-90° C., add 3-5 parts of nuclear monomer dropwise within 10-20 minutes, and keep warm for 10-40 minutes to obtain a seed emulsion;

[0016] S2, add 38-52 parts of core monomer, 1-6 parts of emulsifier, 1-2 parts of initiator, and 1-8 parts of water to the S1 seed emulsion, the adding time is 1-3 hours, and the temperature is kept at 75-90° C. for 10-50 minutes after the adding, to obtain a core layer emulsion;

[0017] S3, add 5-17 parts of shell monomer, 3-16 parts of modifier, 1-6 parts of initiator, and 1-4 parts of water to the S2 core layer emulsion, the adding time is 2-5 hours, and the temperature is kept at 75-90° C. for 1-2 hours after the adding, to obtain a core-shell layer emulsion;

[0018] S4. Cool the S3 core-shell emulsion to 25-38°C, adjust the pH to 8-9 with aqueous ammonia, and filter out the precipitate to obtain a modified emulsion.

[0019] Preferably, the core monomer is any one of sorbitol pentaacrylate, cinnamyl methacrylate, 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, and ethoxypropyl acrylate.

[0020] More preferably, the core monomer is 1,6-bis(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane.

[0021] Preferably, the modifier is 6-vinyl-6-(2-methoxy-1-methylethoxy)-4,8-dimethyl-2,5,7,10-tetraoxa-6-silane.

[0022] Preferably, the shell monomer is hexahydro-4,7-methylene-1H-indenyl acrylate.

[0023] Preferably, the initiator is diisopropyl azodicarboxylate.

[0024] Preferably, the emulsifier is a mixture of sodium lauryl sulfate and octylphenol polyoxyethylene ether.

[0025] A method for preparing decorative paper with low ink consumption comprises the following steps, measured in parts by weight:

[0026] Step 1, mixing 2-10 parts of the modified latex and 5-20 parts of molten polypropylene to obtain a mixed coating;

[0027] Step 2: Take the mixed coating in step 1, fix the filter paper on the glass plate by rod coating, apply the coating on the filter paper, place the coated paper sample in an oven at 95-105°C, and dry for 10-15 minutes to obtain environmentally friendly decorative paper.

[0028] In this recipe, the ingredients and their functions are as follows:

[0029] Emulsifier: Emulsifier is one of the most important components for preparing modified emulsions and emulsion polymerization. The type and amount of emulsifier have a crucial impact on emulsion polymerization and emulsion polymerization products. The emulsification and solubilization effect of emulsifier in emulsion polymerization system maintains the stability of the system. The emulsification effect is mainly reflected in that when there is an emulsifier in the water phase, a layer of emulsifier will be adsorbed on the surface of the monomer droplets added to the water, making it difficult for the monomers to collide into large droplets, thus forming an emulsion state.

[0030] Initiator: Initiator is an indispensable component in the polymerization process of preparing modified latex. In the process of free radical addition polymerization, the initiator first generates initial free radicals, which then react with monomers to generate monomer free radicals. The monomer free radicals further react with monomers to extend the chain and finally generate long-chain macromolecules.

[0031] Buffer: The main function of the buffer is to maintain the stability of the pH value during the reaction. In the process of preparing the modified emulsion, each chemical reaction needs to be carried out under certain pH conditions. If the pH value is unstable, it may lead to problems such as a decrease in reaction rate, incomplete reaction, or changes in the properties of the product. Therefore, by adding a buffer, the pH value during the reaction can be effectively stabilized, ensuring the smooth progress of the reaction, and ultimately obtaining a modified emulsion with stable performance.

[0032] Water: By adding buffer and water, the pH value in the reaction process can be effectively adjusted to ensure that the reaction is carried out under the optimal pH conditions. At the same time, in the process of preparing the modified emulsion, the shell monomer and the modifier are added by dropwise addition, and water helps dilute and flow these substances, making the dropwise addition operation smoother.

[0033] Core monomer: The hydrophilicity of the core monomer is an important factor affecting the structure of the core-shell latex particles. In order to be enriched in the shell layer of the latex particles, a certain hydrophobicity will be selected. The core monomer is the starting point for initiating the polymerization reaction. During the emulsion polymerization process, the core monomer first forms the core of the latex particle, that is, the seed emulsion, and then other components such as shell monomers, modifiers, etc. will further polymerize on these cores to form a core layer and a core-shell structure. The core monomer is an acrylic monomer with a double bond, and the polymer is synthesized by free radical polymerization under the action of an emulsifier system and an initiator. The core monomer adopts acrylates, and the acrylic emulsion has particularly excellent aging resistance and weather resistance. It is resistant to heat aging and ultraviolet aging, and has excellent antioxidant properties. Secondly, the acrylic emulsion also has good film-forming properties and adhesion, which is conducive to being used as a raw material for preparing decorative paper.

[0034] Shell monomer: Shell monomer has a double bond and a huge non-polar ester alkoxy group. The double bond allows it to undergo free radical polymerization with unsaturated monomers. The steric hindrance of the non-polar ester alkoxy group makes the polymer emulsion have low viscosity, small shrinkage, and excellent water resistance and weather resistance. Shell monomer has a similar molecular structure to polypropylene, so it has a strong intermolecular force with polypropylene molecules. Therefore, the modified emulsion prepared by cross-linking the shell monomer and the core monomer has good adhesion to polypropylene.

[0035] Modifier: The modifier uses organosiloxane, and the double bonds in the organosiloxane and the double bonds in the core monomer undergo free radical polymerization. After the organosiloxane is grafted onto the core monomer polymer molecular chain, it will hydrolyze to generate silanol, which will undergo polycondensation and dehydration reaction during the emulsion film formation process, so that the latex film forms a cross-linked network structure, improving the mechanical properties of the modified emulsion.

[0036] Ammonia water: Ammonia water is a strong base that can neutralize the acidic substances that may be produced during the reaction, thereby stabilizing the pH value of the system within the required range. It mainly plays the role of adjusting the pH value.

[0037] Polypropylene: As one of the raw materials for making decorative paper, polypropylene has many excellent properties: it is one of the lightest synthetic resins; it has good mechanical properties and processing properties; it has good heat resistance, and the continuous use temperature can reach 110-120℃, and it is the general plastic with the best thermal stability; it has a low water absorption rate of only 0.01%; it has good chemical stability and good anti-corrosion properties; it has good electrical insulation and is non-toxic. The good barrier and hot filling properties of polypropylene give the packaging industry or printing industry an advantage.

[0038] Beneficial effects of the present invention:

[0039] 1. Compared with the prior art, the present invention utilizes the double bonds contained in the modifier to react with the double bonds in the core monomer for free radical reaction, and utilizes the low surface energy property of the silicone in the modifier to reduce the surface tension of the modified latex and the surface energy of the latex film, so that the modified latex can better wet the polypropylene material, further shorten the distance between the shell monomer, polypropylene, and the coating material, increase the intermolecular force, and make the prepared decorative paper have better ink adhesion.

[0040] 2. Compared with the existing technology, the shell monomer with double bonds and non-polar groups is cross-linked with the core monomer with double bonds through emulsion polymerization to prepare a core-shell modified latex, so that the core-shell structure of the prepared modified latex is more obvious, the particle size is smaller, and the distribution is more uniform, which is beneficial to improve the mechanical properties of decorative paper. DETAILED DESCRIPTION

[0041] Parameters for specific chemical substances used, sources.

[0042] Hexahydro-4,7-methylene-1H-indenyl acrylate, CAS No.: 33791-58-1.

[0043] Sorbitol pentaacrylate, CAS number: 53123-67-4.

[0044] Cinnamyl methacrylate, CAS number: 31736-34-2.

[0045] 1,6-Bis(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, CAS number: 2264-01-9.

[0046] Ethoxypropyl acrylate, CAS number: 64050-15-3.

[0047] 6-ethenyl-6-(2-methoxy-1-methylethoxy)-4,8-dimethyl-2,5,7,10-tetraoxa-6-silaundecane, CAS No.: 96195-81-2.

[0048] Polypropylene, brand: F780R, Shanghai Qiaowei Chemical Technology Co., Ltd.

[0049] Example 1

[0050] A method for preparing decorative paper with low ink consumption comprises the following steps:

[0051] Step 1: melt 20g of polypropylene at 180°C, add 5g of modified latex, and stir at 200rpm for 30min to obtain a mixed coating;

[0052] Step 2: Take the mixed coating in step 1, fix the filter paper on the glass plate by rod coating method, evenly apply the coating on the filter paper, the coating thickness is 20 μm, place the coated paper sample in an oven at 100°C and dry for 15 minutes to obtain environmentally friendly decorative paper.

[0053] Wherein, the preparation method of the modified emulsion comprises the following steps:

[0054] S1. In a four-necked flask equipped with a condenser, a stirring paddle, a constant pressure dropping funnel and a thermometer, a mixture of 4 g of sodium dodecyl sulfate and 2 g of octylphenol polyoxyethylene ether, 4 g of diisopropyl azodicarboxylate, 2 g of sodium bicarbonate and 25 mL of water were added, stirred at 200 rpm, and the temperature was raised from 25° C. to 80° C., and 5 g of 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane was added dropwise within 15 min, and the mixture was kept at 80° C. for 20 min to obtain a seed emulsion;

[0055] S2, dropwise add 50 g of 1,6-bis(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, 4 g of a mixture of sodium dodecyl sulfate and 2 g of octylphenol polyoxyethylene ether, 2 g of diisopropyl azodicarboxylate, and 7 mL of water to the S1 seed emulsion for 2 h, and keep warm at 80° C. for 30 min after the dropwise addition to obtain a core layer emulsion;

[0056] S3, 15g hexahydro-4,7-methylene-1H-indenyl acrylate, 5g 6-vinyl-6-(2-methoxy-1-methylethoxy)-4,8-dimethyl-2,5,7,10-tetraoxa-6-silane, 3g diisopropyl azodicarboxylate, 2mL water were added dropwise to the S2 core layer emulsion for 3h, and the mixture was kept at 80°C for 2h to obtain a core-shell layer emulsion;

[0057] S4, cooling the S3 core-shell emulsion to 30°C, adjusting the pH to 8 with 20 wt% ammonia water, filtering to remove the precipitate, and obtaining a modified emulsion.

[0058] Example 2

[0059] The difference between Example 2 of the present application and Example 1 is that the 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane in S1 and S2 is replaced by sorbitol pentaacrylate.

[0060] Example 3

[0061] The difference between Example 3 of the present application and Example 1 is that the 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane in S1 and S2 is replaced by cinnamyl methacrylate.

[0062] Example 4

[0063] The difference between Example 4 of the present application and Example 1 is that the 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane in S1 and S2 is replaced by ethoxypropyl acrylate.

[0064] Comparative Example 1

[0065] The difference between Comparative Example 1 of the present application and Example 1 is that the hexahydro-4,7-methylene-1H-indenyl acrylate in S3 is replaced by isobornyl acrylate.

[0066] Comparative Example 2

[0067] The difference between Comparative Example 2 of the present application and Example 1 is that the diisopropyl azodicarboxylate in S1, S2 and S3 is replaced by azobisisobutyronitrile.

[0068] Comparative Example 3

[0069] The difference between Comparative Example 3 of the present application and Example 1 is that the 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane in S1 and S2 is replaced by acrylic acid.

[0070] Comparative Example 4

[0071] The difference between Comparative Example 4 of the present application and Example 1 is that the 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane in S1 and S2 is replaced by methyl methacrylate.

[0072] Comparative Example 5

[0073] The difference between Comparative Example 5 of the present application and Example 1 is that 6-vinyl-6-(2-methoxy-1-methylethoxy)-4,8-dimethyl-2,5,7,10-tetraoxa-6-silane is replaced by vinyltriisopropoxysilane.

[0074] Test Example 1

[0075] Water resistance test: The static contact angle of the film layer of the decorative paper prepared in Examples 1-4 and Comparative Examples 1-5 to water is expressed by a contact angle meter. The water droplet size is 5 μL. The average value is taken after 3 measurements. The test results are shown in Table 1:

[0076] Table 1 Water resistance test results

[0077]

[0078]

[0079] Test Example 2

[0080] Adhesion performance test: The adhesion of ink on decorative paper was tested according to GB / T 9286-1998 "Cross-cut test for paint and varnish film". Wipe the surface of the decorative paper with anhydrous ethanol for 2 minutes to remove surface oil stains and dust. The ink was evenly coated on the decorative paper prepared in Examples 1-4 and Comparative Examples 1-5, and the adhesion was tested by the cross-cut method. Judgment standard: the grade is 0-5. Grade 0: The cut surface is completely smooth and the coating does not fall off at all; Grade 1: The affected range of the cross-cut area is no more than 5%, and there are a few thin flakes of coating separated at the intersection of the cut; Grade 2: The affected range of the cross-cut area is 5-15%, and the coating obviously falls off at the cutting edge or the intersection of the cut; Grade 3: The affected range of the cross-cut area is 15-35%, and part of the coating falls off in large fragments along the cutting edge; Grade 4: The affected range of the cross-cut area is 35-65%, and most or all of the coating of some squares falls off; Grade 5: The affected area of ​​the cross-cut area is significantly greater than 65%. The results are shown in Table 2:

[0081] Table 2 Adhesion test results

[0082]

[0083]

[0084] By comparing with Examples 1-4 and Comparative Examples 1-5, it can be found that the decorative paper prepared in Example 1 has better performance in water resistance and ink adhesion. The difference between Examples 1-4 and Comparative Examples 3 and 4 is that different core monomers are used. The possible reason is that compared with these core monomers, the core monomer in Example 1 has fluorine atoms in addition to the double bond functional groups contained in acrylic acid to react with shell monomers and modifiers. According to the hydrophilicity of the core monomer and its solubility in water, the use of hydrophilic monomers in the emulsion polymerization process tends to transfer to the surface of the emulsion particles, which is conducive to the formation of a positive core-shell structure. Fluorine is an active non-metallic element with extremely strong electronegativity and extremely low polarizability. It is easy to obtain an electron to form a stable structure, and the surface energy of the fluorine-containing polymer is low. The bond energy of the CF bond is large, so the fluorine-containing acrylate polymer has good thermal stability and weather resistance. Fluorine atoms are located on the side chains of the fluorine-containing polymer molecular chain. During the film formation process, fluorine atoms migrate to the air interface and are concentrated on the outside of the molecular chain. Since the radius of fluorine atoms is very small, fluorine atoms can be tightly stacked on the outside of the molecular chain to form a spiral molecular chain structure in which fluorine atoms surround the CC main chain. This phenomenon is called the shielding effect of fluorine atoms, which can give fluorine-containing polymers excellent chemical inertness, corrosion resistance, etc. Therefore, fluorine-containing polymers have self-cleaning, low surface energy, water and oil repellency, anti-sticking and other properties, and the decorative paper prepared in Example 1 exhibits better water resistance.

[0085] Compared with Example 1 and Comparative Example 1, the difference is that different shell monomers are used. The possible reason is that the shell monomer used in Example 1 has other non-polar functional groups in addition to the double bonds in isobornyl acrylate, and factors such as spatial structure and positional relationship cause the difference in water resistance of decorative paper. In the process of preparing the modified emulsion, the double bonds in the shell monomer can undergo free radical polymerization with the unsaturated double bonds in the core monomer, and the steric hindrance of the non-polar group makes the prepared polymer emulsion have low viscosity and small shrinkage, so it has excellent water resistance and weather resistance. The non-polar group of hexahydro-4,7-methylene-1H-indenyl acrylate in Example 1 is similar to the molecular structure of polypropylene, so it has a strong intermolecular effect with the polypropylene molecule, so the prepared decorative paper has good ink adhesion, which can reduce ink consumption.

[0086] The difference between Example 1 and Comparative Example 2 is that different initiators are used. The possible reason is that as an oil-soluble thermal initiator, diisopropyl azodicarboxylate has a lower average reaction heat and is less dangerous, so it is more conducive to the polymer reaction, thereby making the prepared core-shell particles better combined and showing good water resistance.

[0087] Compared with Example 1 and Comparative Example 5, the difference lies in the use of different modifiers. The polymerization stability of the organosilicon monomer to the system during the preparation of the modified emulsion is obviously related to the structure of the functional groups carried by the organosilicon monomer. After the organosiloxane is grafted onto the molecular chain of the acrylic polymer, it will be hydrolyzed to generate silanols. The silanols will undergo a polycondensation and dehydration reaction during the emulsion film formation process, so that the latex film forms a cross-linked network structure. The longer the molecular chain of the functional group, the greater the steric hindrance, and the smaller the polarity, the smaller the solubility of the organosilicon monomer in water, the slower the hydrolysis rate, and therefore, the gel formed by hydrolysis and polycondensation is less, and the polymerization stability of the modified emulsion system is better. The organosilicon monomer used in Example 1 may have a longer molecular chain and a low surface energy functional group. Therefore, the polymer of the prepared modified emulsion is more compact and has a larger molecular weight, thereby showing better water resistance and ink adhesion.

Claims

1. A decorative paper with low ink consumption, characterized in that: include: Modified latex, polypropylene; The preparation method of the modified emulsion comprises the following steps, measured in parts by weight: S1. Add 1-10 parts of emulsifier, 1-8 parts of initiator, 2-9 parts of buffer, and 20-40 parts of water into a reaction kettle, stir, and heat to 75-90° C., add 3-5 parts of nuclear monomer dropwise within 10-20 minutes, and keep warm for 10-40 minutes to obtain a seed emulsion; S2, add 38-52 parts of core monomer, 1-6 parts of emulsifier, 1-2 parts of initiator, and 1-8 parts of water to the S1 seed emulsion, the adding time is 1-3 hours, and the temperature is kept at 75-90° C. for 10-50 minutes after the adding, to obtain a core layer emulsion; S3, add 5-17 parts of shell monomer, 3-16 parts of modifier, 1-6 parts of initiator, and 1-4 parts of water to the S2 core layer emulsion, the adding time is 2-5 hours, and the temperature is kept at 75-90° C. for 1-2 hours after the adding, to obtain a core-shell layer emulsion; S4, cooling the S3 core-shell emulsion to 25-38°C, adjusting the pH to 8-9 with aqueous ammonia, filtering and removing the precipitate to obtain a modified emulsion; The core monomer is any one of sorbitol pentaacrylate, cinnamyl methacrylate, 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane, and ethoxypropyl acrylate; The modifier is 6-vinyl-6-(2-methoxy-1-methylethoxy)-4,8-dimethyl-2,5,7,10-tetraoxa-6-silane; The shell monomer is hexahydro-4,7-methylene-1H-indenyl acrylate.

2. The low ink consumption decorative paper according to claim 1, characterized in that: The core monomer is 1,6-di(acryloyloxy)-2,2,3,3,4,4,5,5-octafluorohexane.

3. The low ink consumption decorative paper according to claim 1, characterized in that: The initiator is diisopropyl azodicarboxylate.

4. The low ink consumption decorative paper according to claim 1, characterized in that: The emulsifier is a mixture of sodium lauryl sulfate and octylphenol polyoxyethylene ether.

5. A method for preparing the low ink consumption decorative paper according to any one of claims 1 to 4, comprising the following steps, calculated in parts by weight: Step 1, mixing 2-10 parts of the modified latex and 5-20 parts of molten polypropylene to obtain a mixed coating; Step 2: Take the mixed coating in step 1, fix the filter paper on the glass plate by rod coating, apply the coating on the filter paper, place the coated paper sample in an oven at 95-105°C, and dry for 10-15 minutes to obtain environmentally friendly decorative paper.

Citation Information

Patent Citations

  • Environment-friendly bathroom compounded decorative paper and manufacturing method thereof

    CN103276631B

  • Hydrophobic dirt-resistant decorative paper and production method thereof

    CN116289332A

  • Polyuria-acrylate emulsion and aqueous gravure ink prepared from same

    CN103641962A