Hollow zeolite catalyst for desorption of CO2 absorption rich liquid and its preparation method and application
By designing the H-ZSM-5 zeolite catalyst with a hollow structure, the problems of high energy consumption of CO2 desorption and catalyst deactivation in the chemical absorption method are solved, and efficient CO2 absorption rich liquid desorption is achieved, reducing the cost of carbon capture.
Patent Information
- Application Number
- CN202410066291.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-01-17
AI Technical Summary
In existing carbon capture technology, the CO2 desorption process of chemical absorption method consumes high energy, resulting in high cost. Moreover, the pore size of the solid acid catalyst does not match the CO2-rich amine molecules, which affects the reaction mass transfer efficiency and leads to catalyst deactivation.
The H-ZSM-5 zeolite catalyst with a hollow structure is designed and prepared through hydrothermal treatment and alkali exchange technology to improve the acidic sites and pore size distribution of the catalyst, adapt to the CO2 rich liquid desorption process, and avoid pore blockage.
The mass transfer rate of CO2 absorption rich liquid desorption is significantly improved, the regeneration energy consumption is reduced, the overall CO2 capture cost is reduced, and the service life of the catalyst is extended.
Smart Images

Figure CN117943104B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of carbon capture and carbon neutralization, and specifically relates to a hollow zeolite catalyst and a preparation method and application thereof. Background Art
[0002] Develop carbon capture and utilization (CCU) technology for end-of-pipe treatment of CO2 emitted from fossil fuel combustion to achieve clean utilization of fossil fuels. Chemical absorption using alcohol amines as absorbents for CO2 capture is currently the most commonly used and commercially mature CCU technology, but this technology faces three major limitations: solution loss, equipment corrosion, and high regeneration energy consumption. Among them, the biggest problem facing the chemical absorption method is the high energy consumption of desorbing carbon dioxide during the regeneration of the absorbent, which accounts for about 70-80% of the operating cost of the carbon dioxide capture process. More than 50% of the heat energy is consumed in the process of heating and evaporation of the solution, resulting in an energy consumption of 3.6-4.0 GJ / tCO2 for desorption of alcohol amines. Such high energy consumption results in a cost of 200-400 yuan per ton of CO2 capture, which greatly limits the industrial application of the chemical absorption method.
[0003] Solid acid catalysts have abundant acid sites, which can accelerate the proton transfer rate of CO2 rich solution desorption process and reduce the desorption reaction heat of carbamate. It is a carbon capture technology with application potential. Patent CN 111715274 discloses a preparation method and application of a heterogeneous catalyst for desorption of CO2 in solution. 2- / Metal oxide H-ZSM-5 is used for desorption of CO2-rich amine solution. Compared with no catalyst, the desorption rate is increased by 35-45%, and it can be recycled for more than 4 times. However, the pore size of commonly used solid acid does not match the molecular dynamics diameter of CO2-rich amine. For example, H-ZSM-5 molecular sieve has a three-dimensional cross-ten-membered ring pore system with pore sizes of 0.53nm*0.56nm and 0.51nm*0.55nm respectively. The commonly used absorbent ethanolamine has a molecular size of 2.8nm*0.38nm. After absorbing CO2, its molecular size will further increase, resulting in a great impact on the mass transfer efficiency of the reaction during the catalytic desorption process, and it is easy to cause the molecular sieve to be blocked and deactivated, and the cycle performance is greatly reduced. Therefore, it is of great practical significance to design and synthesize efficient and stable solid catalysts for CO2 absorption and rich solution regeneration. Summary of the invention
[0004] The purpose of the present invention is to address the deficiencies in the prior art and provide a hollow zeolite catalyst for desorption of CO2 absorption rich liquid, a preparation method and an application thereof. By controllably synthesizing the zeolite catalyst H-ZSM-5 with a hollow structure, the mass transfer rate in the desorption process of CO2 absorption rich liquid is improved, and the problems of rapid catalyst deactivation and pore blockage are solved, so as to further reduce the regeneration energy consumption of CO2 absorption rich liquid and reduce the overall cost of capturing CO2.
[0005] The hollow zeolite catalyst for CO2 absorption and rich liquid desorption provided by the present invention is an H-type ZSM-5 molecular sieve (H-ZSM-5) with a hollow (hollow) structure, in which the molar ratio of silicon oxide to aluminum oxide is (10-200):1, and it has weak acid, strong acid and super acid, with a total acid content of 50-300 μmol / g, and the molar ratio of B acid to L acid is (2.5-3.5):1.
[0006] Furthermore, the hollow zeolite catalyst H-ZSM-5 has a mesoporous structure with a pore size distribution of 2-50 nm. Designing mesopores based on the hollow structure can further increase the pore size of the zeolite, improve the reaction mass transfer efficiency, and avoid catalyst deactivation due to pore blockage.
[0007] The present invention provides an application of the hollow zeolite catalyst (or H-type ZSM-5 molecular sieve (H-ZSM-5) with a hollow structure) in carbon capture and utilization (CCU) and carbon capture and storage (CCS).
[0008] Further, the application is in the desorption of CO2 absorption rich solution. Preferably, the application is as a catalyst in the desorption of CO2 absorption rich solution after CO2 capture using alcohol amines as absorbent. Preferably, the catalyst is added in an amount of 0.5-2% of the CO2 absorption rich solution.
[0009] Furthermore, the application is in the regeneration of absorbent in the process of CO2 capture by chemical absorption method.
[0010] The present invention also provides the combined application of the hollow H-ZSM-5 and alcohol amine chemical absorbent in carbon capture and utilization (CCU) and carbon capture and storage (CCS).
[0011] The present invention also provides a method for preparing the hollow zeolite catalyst H-ZSM-5, comprising the following contents:
[0012] The solid H-ZSM-5 zeolite is hydrothermally treated at 150-170° C. for 1-3 days using an organic alkali solution, and then centrifuged, washed, dried, and calcined at 550-600° C. for 4-6 hours to obtain a hollow H-ZSM-5.
[0013] Furthermore, the organic base is one or a combination of tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and tetrapropylammonium bromide. Preferably, the concentration of the organic base solution is 0.3 mol / L, and the amount of the organic base solution is 5 to 15 mL / g. 固体H-ZSM-5 .
[0014] Furthermore, the solid H-ZSM-5 zeolite is prepared by the following method:
[0015] (1) 10 to 60 parts by weight of ethyl orthosilicate and 20 to 80 parts by weight of deionized water are mixed, stirred at 25 to 50° C. for 1 to 2 hours to completely hydrolyze the ethyl orthosilicate, and then 50 to 100 parts by weight of tetrapropylammonium hydroxide are added. After stirring for 2 hours, the temperature is raised to 80 to 110° C. for hydrothermal treatment for 1 to 3 days, cooled, and a white solution is collected, i.e., seed crystal S-1;
[0016] (2) dissolving a silicon source, an aluminum source and an alkali source in a certain amount of water and mixing with a seed crystal S-1, wherein the mass of the seed crystal is 0.1% to 3% of the mass of silicon dioxide in the silicon source, hydrothermally crystallizing at a temperature of 150 to 170° C. for 1 to 3 days, separating the solid and the liquid, drying and calcining at 500 to 600° C. for 4 to 6 hours to obtain a solid Na-ZSM-5 molecular sieve; exchanging the Na-ZSM-5 nanomolecular sieve with an ammonium nitrate solution three times, centrifuging, washing and drying after the exchange, and then calcining at 500 to 540° C. for 4 to 6 hours to convert the Na-ZSM-5 into an H-ZSM-5 molecular sieve, i.e., solid H-ZSM-5;
[0017] Among them, the molar ratio of silicon source, aluminum source, alkali source and water is 0.1:0.1 / x:(0.01~0.05):(1~8) according to the ratio of SiO2, Al2O3, Na2O and H2O, x is the silicon-aluminum ratio of H-ZSM-5 molecular sieve, and the silicon-aluminum ratio ranges from 10 to 200.
[0018] Furthermore, in the preparation method of the above-mentioned solid H-ZSM-5 zeolite, the silicon source is at least one of tetraethyl orthosilicate, silica sol or white carbon black; the aluminum source is aluminum nitrate, sodium aluminate or aluminum isopropoxide; and the alkali source is sodium hydroxide or tetrapropylammonium hydroxide.
[0019] Furthermore, in the preparation method of the above solid H-ZSM-5 zeolite, the concentration of the ammonium nitrate solution is 0.1 to 0.2 mol / L.
[0020] Furthermore, in order to improve the catalytic effect and service life of the catalyst and avoid problems such as rapid catalyst deactivation and pore blockage, the present invention further adjusts the pore size of the above-mentioned hollow zeolite catalyst H-ZSM-5 to a mesoporous (2 to 50 nm) structure. The preparation method of the mesoporous hollow H-ZSM-5 is as follows:
[0021] The hollow H-ZSM-5 is added to a mixed alkaline solution of an organic base and an inorganic base, stirred evenly, and heated at 40-80°C for 2-6 hours. The product is centrifuged, washed, and dried, and then calcined at 550-600°C for 4-6 hours to obtain mesoporous hollow H-ZSM-5. The size of the mesopore is adjusted according to the concentration of the mixed alkaline solution (adjusted within the mesopore range).
[0022] Furthermore, in the preparation of the above-mentioned mesoporous hollow H-ZSM-5, the organic base is one or a combination of tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, and tetrapropylammonium bromide; the inorganic base is one or a combination of sodium hydroxide and potassium hydroxide.
[0023] Furthermore, in the preparation of the above-mentioned mesoporous hollow H-ZSM-5, the total concentration of the mixed alkali solution of organic alkali and inorganic alkali is 0.1-0.2 mol / L, and the dosage is 5-15 mL / g 中空H-ZSM-5 The molar ratio of organic base / (organic base+inorganic base) is (0.1-1):1.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention prepares zeolites with hollow or mesoporous hollow structures, increases the number of zeolite acid sites, increases the B acid / L acid ratio, improves the catalytic desorption efficiency, expands the pore size, and increases the desorption mass transfer rate, thereby solving the problems of rapid catalyst deactivation and pore blockage, further reducing the regeneration energy consumption of CO2 absorption rich liquid, reducing the overall cost of capturing CO2, and achieving low-energy catalytic desorption of CO2. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Comparison of catalytic cycle stability test results of the catalysts in the examples;
[0027] Figure 2 This is a schematic diagram of the design route of the hollow zeolite of the present invention;
[0028] Figure 3 The microscopic characterization diagrams are of Examples 1, 2, and 4, i.e., solid H-ZSM-5-III (a), hollow H-ZSM-5 (b), and mesoporous hollow H-ZSM-5-II (c);
[0029] Figure 4 NH3-TPD spectra of solid H-ZSM-5; hollow H-ZSM-5; mesoporous hollow H-ZSM-5;
[0030] Figure 5 These are the XRD patterns of solid H-ZSM-5; hollow H-ZSM-5; and mesoporous hollow H-ZSM-5. DETAILED DESCRIPTION
[0031] The present invention is further described below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art may make some non-essential improvements and adjustments to the present invention according to the above-mentioned invention content and implement the invention specifically, which still falls within the scope of protection of the invention.
[0032] Example 1
[0033] (1) Synthesis of Seed Crystal S-1: 50 g of tetraethyl orthosilicate and 30 g of deionized water were mixed and added to a three-necked round-bottom flask and a magnet was placed in it, and the mixture was transferred to a constant temperature water bath; the mixture was stirred at 35°C and 400 rpm for 2 hours to completely hydrolyze the tetraethyl orthosilicate, and then 70 g of tetrapropylammonium hydroxide was added, and the mixture was stirred for 2 hours, and then a serpentine condenser was installed. Finally, the temperature was set to 80°C for hydrothermal treatment for 3 days, and the white solution was collected after cooling, which was the Seed Crystal S-1.
[0034] (2) Preparation of solid H-ZSM-5 zeolite: Sodium aluminate and sodium hydroxide are dissolved in a certain amount of water, and gradually dripped into the silica sol under stirring, and finally the seed crystal S-1 is dripped, and hydrothermal crystallization is carried out at a temperature of 170°C for 3 days, centrifugal drying overnight, grinding and roasting at 540°C for 6 hours to obtain solid Na-ZSM-5 zeolite. After exchanging the solid Na-ZSM-5 zeolite with 0.2 mol / L ammonium nitrate solution three times, washing, filtering, drying overnight, and roasting at 500°C for 4 hours to obtain solid H-ZSM-5 zeolite. The molar ratio of SiO2, Al2O3, Na2O, and H2O is 0.1:0.1 / 25:0.02:4 respectively, the silicon-aluminum ratio is 25, and the mass of the seed crystal is 1% of the mass of silicon dioxide in the silicon source.
[0035] Effect test experimental method:
[0036] The desorption and regeneration performance of alcohol amines were evaluated using a self-made CO2 absorption and desorption integrated device. The absorption used a mass flow meter to simulate the flue gas composition (15% CO2-85% N2), and the desorption used a fixed flow of N2 as a carrier. The mixed gas of absorption / desorption passed through the condensation and drying tube and then entered the CO2 concentration and flow sensor for analysis. The temperature rise of the CO2 absorption rich liquid was controlled by an oil bath, and magnetic stirring was used to ensure full contact between the catalyst and the CO2 absorption rich liquid.
[0037] 1. Absorption experiment
[0038] 500 ml of 30% ethanolamine aqueous solution was used to simulate low-concentration CO2 flue gas with N2 / CO2 mixed gas (85 Vol.% / 15 Vol.%), and the absorption rich liquid with a CO2 loading of 0.52 mol CO2 / mol MEA was obtained.
[0039] The CO2 absorption rate and CO2 loading of the organic alcohol amine solution were calculated according to equations (1) and (2).
[0040]
[0041]
[0042] In the formula, is the rate at which the solution absorbs CO2, ml / min; is the N2 inlet rate, 100 mL / min; a is the CO2 concentration percentage at the outlet; is the volume of CO2 absorbed by the solution during time t, mL; t is time, min.
[0043] 2. Desorption experiment
[0044] 0.52 mol CO2 / mol MEA absorption rich solution was added to the reaction bottle, and the catalysts described in the comparative example and the embodiment were added respectively, and the addition amount was 2% of the mass of the MEA absorption rich solution; the blank was thermal desorption without adding catalyst. The desorption temperature was 80-100°C and the desorption time was 90 min.
[0045] The CO2 flue gas analyzer in the device is used to measure the concentration of CO2 during the desorption process, and the rate and amount of CO2 desorption catalyzed by the metal-zeolite are calculated using equations (3) and (4).
[0046]
[0047]
[0048] In the formula, is the amount of CO2 desorbed from the solution within time t, mmol; V des is the CO2 desorption rate of the solution, mmol / s; χ is the CO2 concentration percentage at the desorption outlet.
[0049] 3. Calculation of energy consumption for CO2 desorption
[0050] The evaluation parameter of the catalyst's catalytic CO2 desorption performance is the desorption energy consumption per unit mole of CO2, H (kJ / mol), which is defined as the ratio of the energy input rate to the CO2 desorption rate and is calculated by the following formula (5):
[0051]
[0052] Here E refers to the amount of electricity consumed by CO2 desorption within a certain period of time as recorded by the energy meter. The unit is kW·h and it needs to be converted into kJ when used.
[0053] Since the CO2 desorption energy consumption calculated by this method is only a relative value, in order to better evaluate the catalytic CO2 desorption performance of the catalyst, this project proposed and defined the parameter of relative desorption energy consumption RH (%), taking the desorption energy consumption of blank alcohol amine solution regenerated for 90 minutes as the benchmark (H b , kJ / mol), and its RH is 100%, then the RH of the catalytic CO2 desorption process is the desorption energy consumption H for catalytic CO2 desorption for 90 min. i (kJ / mol) and H b The ratio is calculated by the following formula (6):
[0054]
[0055] 4. Cycle experiment
[0056] After the desorption experiment, the CO2 absorption lean solution was cooled to room temperature, and CO2 was introduced again for absorption saturation and then desorption-absorption-desorption cycle was repeated 10 times.
[0057] Example 2
[0058] Solid H-ZSM-5 was prepared according to the method of Example 1. The solid H-ZSM-5 zeolite was hydrothermally treated with 0.3 mol / L tetrapropylammonium hydroxide solution at 170°C for 3 days. The amount of organic base used was 10 mL / g 固体H-ZSM-5 The obtained sample was centrifuged, washed, dried and then calcined at 550°C for 6h to obtain hollow H-ZSM-5.
[0059] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.
[0060] Example 3
[0061] Hollow H-ZSM-5 was prepared according to the method of Example 2, and the hollow H-ZSM-5 was treated with a mixed alkaline solution of an organic base tetrapropylammonium bromide and an inorganic base sodium hydroxide, and the hollow H-ZSM-5 was added to a 0.1 mol / L mixed alkaline solution, wherein the molar ratio of tetrapropylammonium bromide / (tetrapropylammonium bromide+sodium hydroxide) was 0.6:1, and the amount of the mixed alkaline solution was 15 mL / g 中空H-ZSM-5 The mixture was stirred in a beaker and heated at 60°C for 2 h. The product was centrifuged, washed, dried, and calcined at 550°C for 6 h to obtain mesoporous hollow H-ZSM-5-Ⅰ.
[0062] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.
[0063] Example 4
[0064] Hollow H-ZSM-5 was prepared according to the method of Example 2, and the hollow H-ZSM-5 was treated with a mixed alkaline solution of an organic base tetrapropylammonium bromide and an inorganic base sodium hydroxide, and the hollow H-ZSM-5 was added to a 0.15 mol / L mixed alkaline solution, wherein the molar ratio of tetrapropylammonium bromide / (tetrapropylammonium bromide+sodium hydroxide) was 0.6:1, and the amount of the mixed alkaline solution was 10 mL / g 中空H-ZSM-5 The mixture was stirred and heated in a beaker at 60°C for 2 h, and the product was centrifuged, washed, dried, and calcined at 550°C for 6 h to obtain mesoporous hollow H-ZSM-5-II.
[0065] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.
[0066] Example 5
[0067] Hollow H-ZSM-5 was prepared according to the method of Example 2, and the hollow H-ZSM-5 was treated with a mixed alkaline solution of an organic base tetrapropylammonium bromide and an inorganic base sodium hydroxide, and the hollow H-ZSM-5 was added to a 0.2 mol / L mixed alkaline solution, wherein the molar ratio of tetrapropylammonium bromide / (tetrapropylammonium bromide+sodium hydroxide) was 0.6:1, and the amount of the mixed alkaline solution was 5 mL / g 中空H-ZSM-5 The mixture was stirred and heated in a beaker at 60°C for 2 h, and the product was centrifuged, washed, dried, and calcined at 550°C for 6 h to obtain mesoporous hollow H-ZSM-5-Ⅲ.
[0068] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.
[0069] Comparative Example 1
[0070] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1, but without adding a catalyst.
[0071] Comparative Example 2
[0072] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1, and a commercial zeolite is purchased for comparison, which is denoted as commercial H-ZSM-5.
[0073] Comparative Example 3
[0074] According to the method of Example 2, hollow H-ZSM-5 was prepared, and the hollow H-ZSM-5 was treated with an organic base tetrapropylammonium bromide solution, and the hollow H-ZSM-5 was added to a 0.15 mol / L alkaline solution. The amount of alkaline solution was 10 mL / g 中空H-ZSM-5 The mixture was stirred and heated in a beaker at 60°C for 2 h, and the product was centrifuged, washed, dried, and calcined at 550°C for 6 h to obtain mesoporous hollow H-ZSM-5-Ⅳ.
[0075] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.
[0076] Comparative Example 4
[0077] Hollow H-ZSM-5 was prepared according to the method of Example 2, and the hollow H-ZSM-5 was treated with an inorganic base sodium hydroxide solution, and the hollow H-ZSM-5 was added to a 0.2 mol / L alkaline solution. The amount of the mixed alkaline solution was 10 mL / g 中空H-ZSM-5 The mixture was stirred and heated in a beaker at 60°C for 2 h, and the product was centrifuged, washed, dried, and calcined at 550°C for 6 h to obtain mesoporous hollow H-ZSM-5-V.
[0078] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.
[0079] Table 1 Comparison of relative desorption energy consumption of catalysts in the examples
[0080]
[0081] Note: The average size of mesopores was obtained from TEM images. The total acid content was calculated based on the NH3-TPD spectrum.
[0082] As can be seen from the above table, compared with traditional thermal desorption (blank), the addition of solid H-ZSM-5 catalyst significantly reduces the desorption energy consumption of CO2 absorption rich liquid. Further design and synthesis of hollow zeolite, the acid content and B / L value are improved, which effectively improves the efficiency of catalytic CO2 desorption and reduces the desorption energy consumption. When treated with organic base, the mesopore size is limited due to insufficient alkalinity. When treated with inorganic base, the alkalinity is too high, which destroys the zeolite skeleton structure and affects the catalytic performance. Therefore, by controlling the concentration and dosage of the mixed base, the mesopore size and acid content are adjusted to optimize the hollow structure and size of the hollow zeolite. When the mixed base concentration is 0.15mol / L, the desorption performance of the mesopore hollow H-ZSM-5-II is the best.
[0083] One of the main advantages of solid catalysts is that they can be recycled, thereby reducing the cost of using the catalyst. The cyclic stability of the catalyst is an important parameter for evaluating its performance. Therefore, the CO2 absorption rich liquid regeneration process of the example catalyst was tested for 10 cycles. Figure 1 It can be seen that after 10 cycles, the catalytic desorption performance of the unmodified solid H-ZSM-5 was greatly reduced, with a performance loss of about 13.4%; after the solid H-ZSM-5 was hollowed out, the catalytic stability was improved, with a performance loss of about 8.2%. By further optimizing the mesopore size of the hollow H-ZSM-5, the performance of the mesopore hollow H-ZSM-5-II was only lost by 4.6% after 10 cycles, maintaining good cycle stability.
[0084] Solid H-ZSM-5 is prepared by hydrothermal synthesis, and on this basis, alkali treatment is performed to prepare hollow H-ZSM-5. Further treatment with organic alkali, inorganic alkali and a mixture of the two can control the alkali concentration, alkali dosage, treatment time and temperature to prepare mesoporous hollow H-ZSM-5. Figure 3 The microscopic characterization diagrams are of solid H-ZSM-5 (Example 1); hollow H-ZSM-5 (Example 2); and mesoporous hollow H-ZSM-5 (Example 3). Figure 3 It can be seen that H-ZSM-5 changes from solid zeolite to hollow zeolite and then to mesoporous hollow zeolite. The results of NH3-TPD quantitative analysis of solid H-ZSM-5, hollow H-ZSM-5 and mesoporous hollow H-ZSM-5 are as follows: Figure 4 .from Figure 4 It can be seen that the total acid content of hollow and mesoporous H-ZSM-5 is greatly increased.
[0085] Table 3 Changes in total acid content and B acid and L acid before and after zeolite treatment
[0086]
[0087] a: The number of acid sites in the sample was calculated based on the NH3-TPD spectrum and infrared spectrum after pyridine desorption at 150°C.
[0088] The changes in the contents of L acid and B acid before and after treatment of solid H-ZSM-5, hollow H-ZSM-5, and mesoporous hollow H-ZSM-5 were further analyzed by pyridine infrared, and the results are shown in Table 3. As can be seen from Table 3, the increase in the acid content of hollow and mesoporous hollow H-ZSM-5 is mainly due to the increase in B acid content, which can enhance the desorption of carbamate (Amine - COO - )’s fracture. Figure 5 The XRD patterns of solid H-ZSM-5, hollow H-ZSM-5, and mesoporous hollow H-ZSM-5 are shown in Figure 2. Figure 5 It can be seen that all samples have diffraction peaks at 7.9°, 8.8°, 23.1°, 23.9° and 24.3°, showing the typical MFI topological structure of H-ZSM-5.
Claims
1. A hollow zeolite catalyst for desorption of CO2 absorbed rich liquid, characterized in that: The hollow zeolite catalyst is an H-type ZSM-5 molecular sieve with a hollow structure, wherein the molar ratio of silicon oxide to aluminum oxide is (10-200):1, and the molar ratio of B acid to L acid is (2.5-3.5):1; the hollow zeolite catalyst is a mesoporous hollow zeolite catalyst with an average mesopore size of 5-25 nm; The catalyst is prepared by the following method: The solid H-ZSM-5 zeolite is hydrothermally treated with an organic alkali solution at 150-170°C for 1-3 days, and then centrifuged, washed, dried, and calcined at 550-600°C for 4-6 hours to obtain a hollow zeolite catalyst H-ZSM-5; The hollow H-ZSM-5 is added to a mixed alkaline solution of an organic base and an inorganic base, stirred evenly, and heated at 40-80°C for 2-6 hours. The product is centrifuged, washed, and dried, and then calcined at 550-600°C for 4-6 hours to obtain mesoporous hollow H-ZSM-5.
2. Application of the hollow zeolite catalyst according to claim 1 in the fields of carbon capture and utilization, and carbon capture and storage.
3. Use of the hollow zeolite catalyst according to claim 1 in the regeneration of chemical absorbent in CO2 capture and / or the desorption of CO2 absorbed rich liquid by chemical absorption method.
4. The combined use of the hollow zeolite catalyst according to claim 1 and the alcohol amine CO2 chemical absorbent in carbon capture and utilization, and carbon capture and storage.
5. The method for preparing the hollow zeolite catalyst according to claim 1, characterized in that: Includes the following: The solid H-ZSM-5 zeolite is hydrothermally treated with an organic alkali solution at 150-170°C for 1-3 days, and then centrifuged, washed, dried, and calcined at 550-600°C for 4-6 hours to obtain a hollow zeolite catalyst H-ZSM-5; The hollow H-ZSM-5 is added to a mixed alkali solution of an organic base and an inorganic base, stirred evenly, and heated at 40-80°C for 2-6 hours, the product is centrifuged, washed, dried, and then calcined at 550-600°C for 4-6 hours to obtain mesoporous hollow H-ZSM-5; The organic base is one or a combination of tetrapropylammonium hydroxide, tetrabutylammonium hydroxide and tetrapropylammonium bromide; The solid H-ZSM-5 zeolite is prepared by the following method: (1) 10-60 parts by weight of ethyl orthosilicate and 20-80 parts by weight of deionized water are mixed, stirred at 25-50° C. for 1-2 hours to completely hydrolyze the ethyl orthosilicate, and then 50-100 parts by weight of tetrapropylammonium hydroxide are added. After stirring for 2 hours, the temperature is raised to 80-110° C. for hydrothermal treatment for 1-3 days, cooled, and the white solution is collected, i.e., the seed crystal S-1; (2) dissolving a silicon source, an aluminum source and an alkali source in a certain amount of water and mixing with a seed crystal S-1, wherein the mass of the seed crystal is 0.1% to 3% of the mass of silicon dioxide in the silicon source, and hydrothermally crystallizing at a temperature of 150 to 170°C for 1 to 3 days, separating the solid and the liquid, drying and calcining at 500 to 600°C for 4 to 6 hours to obtain a solid Na-ZSM-5 molecular sieve; exchanging the Na-ZSM-5 nanomolecular sieve with an ammonium nitrate solution three times, centrifuging, washing and drying after the exchange, and then calcining at 500 to 540°C for 4 to 6 hours to convert the Na-ZSM-5 into an H-ZSM-5 molecular sieve, i.e., solid H-ZSM-5; Among them, the molar ratio of the silicon source, aluminum source, alkali source and water is 0.1: 0.1 / x: (0.01~0.05): (1~8) according to the ratio of SiO2, Al2O3, Na2O, H2O, x is the silicon-aluminum ratio of the H-ZSM-5 molecular sieve, and the silicon-aluminum ratio ranges from 10 to 200.
6. The method according to claim 5, characterized in that: The silicon source is at least one of tetraethyl orthosilicate, silica sol or white carbon black; the aluminum source is aluminum nitrate, sodium metaaluminate or aluminum isopropoxide; and the alkali source is sodium hydroxide or tetrapropylammonium hydroxide.
Citation Information
Patent Citations
Preparation method and application of heterogeneous catalyst for desorbing CO2 in solution
CN111715274A
Method for preparing hollow zeolite socony mobil-5 (ZSM-5) nanometer zeolite
CN102491366A
Hollow H-ZSM-5 molecular sieve, and preparation method and application thereof
CN105036152A
Preparation method of oxide-molecular sieve catalyst
CN108246345A
Application of oxide-molecular sieve catalyst in catalyzing carbon dioxide desorption
CN108392950A