A high-strength and high-toughness carbon ceramic brake disc and preparation method thereof

By staggered stacking of carbon fiber unidirectional cloth layers and chopped carbon fiber layers, combining chemical vapor deposition and silicon permeability processes, the problem of easy corrosion of the carbon ceramic brake disc mesh tire layer fibers is solved, significantly improving the strength and toughness of the brake discs, satisfying the satisfaction of High performance needs of modern transportation.

CN117962432BActive Publication Date: 2024-12-06深圳市佰斯倍新材料科技有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311810225.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-12-06
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

During the preparation process of existing carbon ceramic brake discs, the fibers of the mesh tire layer are easily corroded by silicon, resulting in insufficient strength and toughness, which cannot meet the high-performance demand of modern transportation tools for brake disc performance.

Method used

The staggered stacked carbon fiber unidirectional cloth layer and chopped carbon fiber layer structure are adopted to optimize the matrix structure and process flow of the brake disc through chemical vapor deposition and silicon permeation processes, increase the protection effect of carbon fibers, and improve the overall strength and toughness of the brake disc.

Benefits of technology

It effectively avoids the problem of strength reduction caused by silicone permeation, significantly improves the overall strength and toughness of the brake disc, and meets high-performance needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117962432B_ABST
    Figure CN117962432B_ABST
Patent Text Reader

Abstract

The present invention provides a high-strength and high-toughness carbon ceramic brake disc, wherein the brake disc blank of the high-strength and high-toughness carbon ceramic brake disc comprises N carbon fiber unidirectional cloth layers and N short-cut carbon fiber layers, wherein the carbon fiber unidirectional cloth layers and the short-cut carbon fiber layers are staggered and stacked, wherein the carbon fiber unidirectional cloth layers have a thickness of 0.4-0.8 mm, and the short-cut carbon fiber layers have a thickness of 0.5-1 mm. By optimizing the brake disc blank structure and alternately arranging the carbon fiber unidirectional cloth layers and the short-cut carbon fiber layers, the overall strength and toughness of the brake disc can be further improved compared with the combination of ordinary carbon fiber unidirectional cloth and mesh tire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of brake disc manufacturing, and in particular to a high-strength and high-toughness carbon ceramic brake disc and a preparation method thereof. Background Art

[0002] Braking materials for modern vehicles like airplanes, automobiles, and high-speed trains have evolved from cast iron, synthetic materials, and powder metallurgy materials to carbon-carbon and carbon-ceramic composites. Both carbon-carbon and carbon-ceramic brake discs offer superior performance compared to cast iron discs. With the rapid development of the transportation industry, vehicle braking performance requirements have also increased. Furthermore, as friction material surfaces shrink, the energy per unit area required increases, placing even higher demands on the strength and toughness of brake discs.

[0003] Currently, carbon-ceramic brake discs are mostly manufactured using a combination of unidirectional cloth and mesh. A multi-layer needle punching process is used to obtain a carbon fiber blank, which is then subjected to high-temperature treatment, chemical vapor deposition, high-temperature treatment, and siliconization to obtain a carbon-ceramic brake disc. A mesh layer exists between the continuous fibers, and most of the fibers in the mesh layer exist as single fibers. Even after chemical vapor deposition, the carbon fibers are easily corroded by silicon, resulting in low sample strength. This results in the inability to effectively improve the overall strength of the entire brake disc. Therefore, a high-strength and high-toughness carbon-ceramic brake disc is proposed to meet the current high-performance requirements of brake discs. Summary of the Invention

[0004] The purpose of the present invention is to provide a high-strength and high-toughness carbon ceramic brake disc and a preparation method thereof, and to improve the strength and toughness of the brake disc by optimizing the brake disc matrix structure and process technology.

[0005] To achieve this object, the present invention provides a high-strength and high-toughness carbon-ceramic brake disc, the brake disc blank of which includes N carbon fiber unidirectional cloth layers and N short-cut carbon fiber layers, where N is a natural number greater than 1, and the carbon fiber unidirectional cloth layers and the short-cut carbon fiber layers are staggered and stacked. The thickness of the carbon fiber unidirectional cloth layers is 0.4-0.8mm, and the thickness of the short-cut carbon fiber layers is 0.5-1mm.

[0006] Preferably, the carbon fiber unidirectional cloth layer comprises a plurality of unidirectional carbon fiber bundles, and the interval between two adjacent unidirectional carbon fiber bundles is 1-4 mm.

[0007] Preferably, the unidirectional carbon fiber bundle is a 4-12K carbon fiber bundle.

[0008] Preferably, the carbon fiber bundles of the chopped carbon fibers in the chopped carbon fiber layer are 2-8K.

[0009] Preferably, the length of the chopped carbon fibers in the chopped carbon fiber layer is 5-15 mm.

[0010] Preferably, the outer surface of the chopped carbon fibers included in the chopped carbon fiber layer is coated with a deposited carbon layer, and the thickness of the deposited carbon layer is 0.5-1.5 μm.

[0011] Preferably, the high-strength and high-toughness carbon-ceramic brake disc contains 40-55% silicon carbide, 45-60% carbon and 4-15% silicon.

[0012] The present invention also provides a method for preparing a high-strength and high-toughness carbon-ceramic brake disc. The method for preparing the high-strength and high-toughness carbon-ceramic brake disc is as follows:

[0013] Step 1: chemical vapor deposition of carbon fibers and cutting the deposited carbon fibers to a predetermined length;

[0014] Step 2: Take several sheets of carbon fiber unidirectional cloth and place them in a mold in a combination of a carbon fiber unidirectional cloth and a layer of chopped carbon fiber until a stacked carbon fiber body of a predetermined thickness is obtained;

[0015] Step 3: Impregnation treatment of the stacked carbon fiber body;

[0016] Step 4: Drying the impregnated stacked carbon fiber body;

[0017] Step 5: hot-pressing the dried stacked carbon fiber body, and removing the mold after the hot-pressing treatment to obtain a hot-pressed carbon fiber blank;

[0018] Step 6: Carbonizing the hot-pressed carbon fiber blank;

[0019] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank;

[0020] Step 8: Place the brake disc blank into a boron nitride crucible and place it in a high-temperature vacuum furnace for siliconizing treatment;

[0021] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the carbon-ceramic brake disc.

[0022] Preferably, in step 1, the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of each layer of chopped carbon fiber layer form an angle of 90°.

[0023] Preferably, the chemical vapor deposition conditions in step 1 are: methane flow rate of 80-180 L / h, nitrogen flow rate of 3-20 L / h, deposition temperature of 950-1100° C., and deposition time of 80-200 h.

[0024] Preferably, the impregnation liquid in step 3 is a 30-50 wt % phenolic resin alcohol solution.

[0025] Preferably, in step 5, the temperature of the hot press is 150° C., the pressure is 3-10 MPa, and the hot pressing time is 4 hours.

[0026] Preferably, the carbonization temperature in step 6 is 1000°C.

[0027] Preferably, in step 8, the boron nitride crucible is pre-placed with pure silicon powder having a mass 1.1 times that of the brake disc blank.

[0028] Preferably, in step 8, the siliconizing treatment temperature is 1600-1700° C., the holding time is 2-4 hours, and the furnace pressure is less than 1000 Pa.

[0029] Beneficial effects: The high-strength and high-toughness carbon-ceramic brake disc provided by the present invention can further improve the overall strength and toughness of the brake disc compared to the combination of ordinary carbon fiber unidirectional cloth and mesh tire by optimizing the brake disc blank structure and alternatingly arranging carbon fiber unidirectional cloth layers and short-cut carbon fiber layers. Since the short-cut carbon fiber bundle contains a large amount of carbon fiber filaments, the carbon fiber is not easily corroded by liquid silicon during siliconization, and still maintains good strength and toughness after siliconization, which can effectively solve the problem of low strength and poor toughness of the mesh tire layer after siliconization. In addition, the carbon fiber in the short-cut fiber layer of the carbon-ceramic brake disc undergoes chemical vapor deposition, which has a better protective effect on the carbon fiber during siliconization, effectively avoiding the problem of strength reduction caused by siliconization. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a schematic structural diagram of the high-strength and high-toughness carbon ceramic brake disc of the present invention.

[0031] Figure 2 This is a schematic diagram of the side structure of the brake disc blank.

[0032] In the figure: 1-brake disc blank, 2-chopped carbon fiber layer, 3-carbon fiber unidirectional cloth layer. DETAILED DESCRIPTION

[0033] The embodiments described below are only some of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0034] This embodiment provides a high-strength and high-toughness carbon-ceramic brake disc. The brake disc blank of the high-strength and high-toughness carbon-ceramic brake disc includes N unidirectional carbon fiber cloth layers and N chopped carbon fiber layers, the unidirectional carbon fiber cloth layers and the chopped carbon fiber layers being stacked alternately. The unidirectional carbon fiber cloth layers have a thickness of 0.4-0.8 mm, and the chopped carbon fiber layers have a thickness of 0.5-1 mm. N is a natural number greater than 1.

[0035] refer to Figure 1 and Figure 2 The bottom of the brake disc blank 1 is a chopped carbon fiber layer 2, and the upper layer of the chopped carbon fiber layer 2 is a carbon fiber unidirectional cloth layer 3. The upper layer of the carbon fiber unidirectional cloth layer 3 is a second chopped carbon fiber layer 2, and the upper layer of the second chopped carbon fiber layer 2 is a second carbon fiber unidirectional cloth layer 3. The brake disc blank 1 is stacked in this manner, and the top of the brake disc blank 1 is the chopped carbon fiber layer 2. The brake disc blank 1 has a total of five layers of chopped carbon fiber layers 2 and four layers of carbon fiber unidirectional cloth layers 3.

[0036] The carbon fiber unidirectional cloth layer includes a plurality of unidirectional carbon fiber bundles, and the interval between two adjacent unidirectional carbon fiber bundles is 1-4 mm.

[0037] The unidirectional carbon fiber bundle is a 4-12K carbon fiber bundle.

[0038] The carbon fiber bundles of the chopped carbon fibers in the chopped carbon fiber layer are 2-8k.

[0039] The length of the chopped carbon fibers in the chopped carbon fiber layer is 5-15 mm.

[0040] The outer surface of the chopped carbon fibers in the chopped carbon fiber layer is a deposited carbon layer, and the thickness of the deposited carbon layer is 0.5-1.5 μm.

[0041] The high-strength and high-toughness carbon-ceramic brake disc contains 40-55% silicon carbide, 45-60% carbon and 4-15% silicon.

[0042] The preparation method of the high-strength and high-toughness carbon ceramic brake disc is as follows:

[0043] Step 1: chemical vapor deposition of carbon fibers and cutting the deposited carbon fibers to a predetermined length;

[0044] Step 2: Take several sheets of carbon fiber unidirectional cloth and place them in a mold in a combination of a carbon fiber unidirectional cloth and a layer of chopped carbon fiber until a stacked carbon fiber body of a predetermined thickness is obtained;

[0045] Step 3: Impregnation treatment of the stacked carbon fiber body;

[0046] Step 4: Drying the impregnated stacked carbon fiber body;

[0047] Step 5: hot-pressing the dried stacked carbon fiber body, and removing the mold after the hot-pressing treatment to obtain a hot-pressed carbon fiber blank;

[0048] Step 6: Carbonizing the hot-pressed carbon fiber blank;

[0049] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank;

[0050] Step 8: Place the brake disc blank into a boron nitride crucible and place it in a high-temperature vacuum furnace for siliconizing treatment;

[0051] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the carbon-ceramic brake disc.

[0052] in:

[0053] In step 1, the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of each layer of chopped carbon fiber layer are at a 90° angle.

[0054] The chemical vapor deposition conditions in step 1 are: methane flow rate of 80-180 L / h, nitrogen flow rate of 3-20 L / h, deposition temperature of 950-1100° C., and deposition time of 80-200 h.

[0055] The impregnation liquid in step 3 is a 30-50wt% phenolic resin alcohol solution.

[0056] In step 5, the temperature of the hot press is 150° C., the pressure is 3-10 MPa, and the hot pressing time is 4 h.

[0057] The carbonization temperature in step 6 is 1000°C.

[0058] In step 8, pure silicon powder 1.1 times the mass of the brake disc blank is pre-placed into the boron nitride crucible.

[0059] In step 8, the siliconizing treatment temperature is 1600-1700°C, the holding time is 2-4 hours, and the furnace pressure is less than 1000Pa.

[0060] Example 1

[0061] This embodiment provides a high-strength and high-toughness carbon-ceramic brake disc, the preparation steps of which are as follows:

[0062] Step 1: Chemical vapor deposition is performed on the carbon fiber and the deposited carbon fiber is cut to a predetermined length to obtain chopped carbon fiber. The chemical vapor deposition conditions are: methane flow rate is 100 L / h, nitrogen flow rate is 8 L / h, deposition temperature is 1000°C, and deposition time is 120 h.

[0063] Step 2: Place the carbon fiber unidirectional cloth in a mold of a certain shape, and lay the chopped carbon fiber on the carbon fiber unidirectional cloth with a thickness of 0.5mm. Then lay another layer of carbon fiber unidirectional cloth at a 90° angle to the carbon fiber direction, and stack them in the above manner to the required thickness to obtain a stacked carbon fiber body. The thickness of the carbon fiber unidirectional cloth used is 0.5mm;

[0064] Step 3: impregnating the stacked carbon fiber body in the mold with a 40wt% concentration of phenolic resin alcohol solution;

[0065] Step 4: Dry the impregnated stacked carbon fiber body until the alcohol is completely evaporated;

[0066] Step 5: Place the dried stacked carbon fiber body and the mold into a hot press for hot pressing at a temperature of 150°C, a pressure of 5 MPa, and a time of 4 hours. After the hot pressing treatment, the mold is removed to obtain a hot-pressed carbon fiber blank;

[0067] Step 6: Carbonizing the hot-pressed carbon fiber blank at a carbonization temperature of 1000°C;

[0068] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank, and prepare features such as ventilation ducts of the product;

[0069] Step 8: Place the brake disc blank into a boron nitride crucible and place it into a high-temperature vacuum furnace for siliconizing treatment. 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the holding time is 2 hours, and the furnace pressure is less than 1000Pa.

[0070] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the high-strength and high-toughness carbon ceramic brake disc.

[0071] Example 2

[0072] This embodiment provides a high-strength and high-toughness carbon-ceramic brake disc, the preparation steps of which are as follows:

[0073] Step 1: Chemical vapor deposition is performed on the carbon fiber and the deposited carbon fiber is cut to a predetermined length to obtain chopped carbon fiber. The chemical vapor deposition conditions are: methane flow rate is 100 L / h, nitrogen flow rate is 8 L / h, deposition temperature is 1000°C, and deposition time is 120 h.

[0074] Step 2: Place the carbon fiber unidirectional cloth in a mold of a certain shape, and lay the chopped carbon fiber on the carbon fiber unidirectional cloth with a thickness of 0.9mm. Then lay another layer of carbon fiber unidirectional cloth at a 90° angle to the carbon fiber direction, and stack them in the above manner to the required thickness to obtain a stacked carbon fiber body. The thickness of the carbon fiber unidirectional cloth used is 0.5mm;

[0075] Step 3: impregnating the stacked carbon fiber body in the mold with a 40wt% concentration of phenolic resin alcohol solution;

[0076] Step 4: Dry the impregnated stacked carbon fiber body until the alcohol is completely evaporated;

[0077] Step 5: Place the dried stacked carbon fiber body and the mold into a hot press for hot pressing at a temperature of 150°C, a pressure of 5 MPa, and a time of 4 hours. After the hot pressing treatment, the mold is removed to obtain a hot-pressed carbon fiber blank;

[0078] Step 6: Carbonizing the hot-pressed carbon fiber blank at a carbonization temperature of 1000°C;

[0079] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank, and prepare features such as ventilation ducts of the product;

[0080] Step 8: Place the brake disc blank into a boron nitride crucible and place it into a high-temperature vacuum furnace for siliconizing treatment. 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the holding time is 2 hours, and the furnace pressure is less than 1000Pa.

[0081] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the high-strength and high-toughness carbon ceramic brake disc.

[0082] Example 3

[0083] This embodiment provides a high-strength and high-toughness carbon-ceramic brake disc, the preparation steps of which are as follows:

[0084] Step 1: Chemical vapor deposition is performed on the carbon fiber and the deposited carbon fiber is cut to a predetermined length to obtain chopped carbon fiber. The chemical vapor deposition conditions are: methane flow rate is 100 L / h, nitrogen flow rate is 8 L / h, deposition temperature is 1000°C, and deposition time is 120 h.

[0085] Step 2: Place the carbon fiber unidirectional cloth in a mold of a certain shape, and lay the chopped carbon fiber on the carbon fiber unidirectional cloth with a thickness of 0.5mm. Then lay another layer of carbon fiber unidirectional cloth at a 90° angle to the carbon fiber direction, and stack them in the above manner to the required thickness to obtain a stacked carbon fiber body. The thickness of the carbon fiber unidirectional cloth used is 0.7mm;

[0086] Step 3: impregnating the stacked carbon fiber body in the mold with a 40wt% concentration of phenolic resin alcohol solution;

[0087] Step 4: Dry the impregnated stacked carbon fiber body until the alcohol is completely evaporated;

[0088] Step 5: Place the dried stacked carbon fiber body and the mold into a hot press for hot pressing at a temperature of 150°C, a pressure of 5 MPa, and a time of 4 hours. After the hot pressing treatment, the mold is removed to obtain a hot-pressed carbon fiber blank;

[0089] Step 6: Carbonizing the hot-pressed carbon fiber blank at a carbonization temperature of 1000°C;

[0090] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank, and prepare features such as ventilation ducts of the product;

[0091] Step 8: Place the brake disc blank into a boron nitride crucible and place it into a high-temperature vacuum furnace for siliconizing treatment. 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the holding time is 2 hours, and the furnace pressure is less than 1000Pa.

[0092] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the high-strength and high-toughness carbon ceramic brake disc.

[0093] Example 4

[0094] This embodiment provides a high-strength and high-toughness carbon-ceramic brake disc, the preparation steps of which are as follows:

[0095] Step 1: Chemical vapor deposition is performed on the carbon fiber and the deposited carbon fiber is cut to a predetermined length to obtain chopped carbon fiber. The chemical vapor deposition conditions are: methane flow rate is 100 L / h, nitrogen flow rate is 8 L / h, deposition temperature is 1000°C, and deposition time is 120 h.

[0096] Step 2: Place the carbon fiber unidirectional cloth in a mold of a certain shape, and lay the chopped carbon fiber on the carbon fiber unidirectional cloth with a thickness of 0.9mm. Then lay another layer of carbon fiber unidirectional cloth at a 90° angle to the carbon fiber direction, and stack them in the above manner to the required thickness to obtain a stacked carbon fiber body. The thickness of the carbon fiber unidirectional cloth used is 0.7mm;

[0097] Step 3: impregnating the stacked carbon fiber body in the mold with a 40wt% concentration of phenolic resin alcohol solution;

[0098] Step 4: Dry the impregnated stacked carbon fiber body until the alcohol is completely evaporated;

[0099] Step 5: Place the dried stacked carbon fiber body and the mold into a hot press for hot pressing at a temperature of 150°C, a pressure of 5 MPa, and a time of 4 hours. After the hot pressing treatment, the mold is removed to obtain a hot-pressed carbon fiber blank;

[0100] Step 6: Carbonizing the hot-pressed carbon fiber blank at a carbonization temperature of 1000°C;

[0101] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank, and prepare features such as ventilation ducts of the product;

[0102] Step 8: Place the brake disc blank into a boron nitride crucible and place it into a high-temperature vacuum furnace for siliconizing treatment. 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the holding time is 2 hours, and the furnace pressure is less than 1000Pa.

[0103] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the high-strength and high-toughness carbon ceramic brake disc.

[0104] Example 5

[0105] This embodiment provides a high-strength and high-toughness carbon-ceramic brake disc, the preparation steps of which are as follows:

[0106] Step 1: Cutting the carbon fiber to a predetermined length to obtain chopped carbon fiber;

[0107] Step 2: Place the carbon fiber unidirectional cloth in a mold of a certain shape, and lay the chopped carbon fiber on the carbon fiber unidirectional cloth with a thickness of 0.5mm. Then lay another layer of carbon fiber unidirectional cloth at a 90° angle to the carbon fiber direction, and stack them in the above manner to the required thickness to obtain a stacked carbon fiber body. The thickness of the carbon fiber unidirectional cloth used is 0.5mm;

[0108] Step 3: impregnating the stacked carbon fiber body in the mold with a 40wt% concentration of phenolic resin alcohol solution;

[0109] Step 4: Dry the impregnated stacked carbon fiber body until the alcohol is completely evaporated;

[0110] Step 5: Place the dried stacked carbon fiber body and the mold into a hot press for hot pressing at a temperature of 150°C, a pressure of 5 MPa, and a time of 4 hours. After the hot pressing treatment, the mold is removed to obtain a hot-pressed carbon fiber blank;

[0111] Step 6: Carbonizing the hot-pressed carbon fiber blank at a carbonization temperature of 1000°C;

[0112] Step 7: Mechanically process the hot-pressed carbon fiber blank to obtain a brake disc blank, and prepare features such as ventilation ducts of the product;

[0113] Step 8: Place the brake disc blank into a boron nitride crucible and place it into a high-temperature vacuum furnace for siliconizing treatment. 1.1 times the mass of the brake disc blank is pre-placed in the boron nitride crucible with pure silicon powder. The siliconizing treatment temperature is 1650°C, the holding time is 2 hours, and the furnace pressure is less than 1000Pa.

[0114] Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the high-strength and high-toughness carbon ceramic brake disc.

[0115] Comparative Example 1

[0116] This comparative example provides a carbon-ceramic brake disc, the brake disc body of which is formed by stacking a carbon fiber unidirectional cloth and a mesh. The preparation method comprises: cross-stacking the carbon fiber unidirectional cloth and the carbon fiber mesh to form a carbon fiber preform; impregnating the carbon fiber preform with a 40 wt% phenolic resin alcohol solution; and drying the impregnated carbon fiber preform until the alcohol is completely volatilized. The dried carbon fiber preform is carbonized at 1000°C for 4 hours. A low-temperature graphitization treatment is then performed to obtain a graphitized body at 1700°C for 2 hours. The graphitized body is then machined to obtain a brake disc body. The brake disc body is placed in a boron nitride crucible containing 1.1 times the mass of pure silicon powder of the brake disc body, and then placed in a high-temperature vacuum furnace for siliconization at 1650°C for 2 hours at a furnace pressure of less than 1000 Pa. The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

[0117] The carbon-ceramic brake discs prepared in Examples 1-4 and Comparative Example 1 were tested for shear strength and bending strength using the test method according to GB / T 15089-2001.

[0118] The test data is shown in Table 1 below.

[0119] Table 1 Test data of carbon ceramic brake discs of Examples 1-4 and Comparative Example 1

[0120]

[0121] The above examples and comparative examples demonstrate that the carbon-ceramic brake disc provided by the present invention, by replacing the conventional mat layer with chopped carbon fibers, can significantly enhance its flexural and shear strength. However, in Example 5, the carbon fibers were not vapor-deposited, and the carbon fibers were not protected by the deposited carbon during the siliconization process. Therefore, the resulting carbon-ceramic brake disc's strength and toughness remain to be improved.

[0122] The above disclosures are merely some preferred embodiments of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the scope of the patent application of the present invention are still within the scope covered by the present invention.

Claims

1. A high-strength and high-toughness carbon ceramic brake disc, characterized in that: The brake disc blank of the high-strength and high-toughness carbon-ceramic brake disc includes N carbon fiber unidirectional cloth layers and N chopped carbon fiber layers, wherein N is a natural number greater than 1, the carbon fiber unidirectional cloth layers and the chopped carbon fiber layers are staggered and stacked, the carbon fiber unidirectional cloth layers have a thickness of 0.4-0.8mm, and the chopped carbon fiber layers have a thickness of 0.5-1mm; the outer surface of the chopped carbon fibers contained in the chopped carbon fiber layers is covered with a deposited carbon layer, and the thickness of the deposited carbon layer is 0.5-1.5μm.

2. The high-strength and high-toughness carbon ceramic brake disc according to claim 1, characterized in that: The carbon fiber unidirectional cloth layer comprises at least two unidirectional carbon fiber bundles, and the interval between two adjacent unidirectional carbon fiber bundles is 1-4 mm.

3. The high-strength and high-toughness carbon ceramic brake disc according to claim 2, characterized in that: The unidirectional carbon fiber bundle is a 4-12K carbon fiber bundle.

4. The high-strength and high-toughness carbon ceramic brake disc according to claim 1, characterized in that: The carbon fiber bundles of the chopped carbon fibers in the chopped carbon fiber layer are 2-8K.

5. The high-strength and high-toughness carbon ceramic brake disc according to claim 4, characterized in that: The length of the chopped carbon fibers in the chopped carbon fiber layer is 5-15 mm.

6. A method for preparing a high-strength and high-toughness carbon ceramic brake disc as claimed in any one of claims 1 to 5, characterized in that: The preparation method of the high-strength and high-toughness carbon ceramic brake disc is as follows: Step 1: chemically vapor depositing carbon fibers and cutting the deposited carbon fibers to a predetermined length; Step 2: Take a number of carbon fiber unidirectional fabrics, and place them in a mold in a combination of a carbon fiber unidirectional fabric and a layer of chopped carbon fiber in an overlapping manner until a stacked carbon fiber body of a predetermined thickness is obtained; Step 3: Impregnating the stacked carbon fiber body; Step 4: Drying the impregnated stacked carbon fiber body; Step 5: hot-pressing the dried stacked carbon fiber body, and removing the mold after the hot-pressing treatment to obtain a hot-pressed carbon fiber blank; Step 6: Carbonizing the hot pressed carbon fiber blank; Step 7: Mechanically process the hot pressed carbon fiber blank to obtain a brake disc blank; Step 8: Place the brake disc blank into a boron nitride crucible and place it into a high-temperature vacuum furnace for siliconizing treatment; Step 9: The siliconized brake disc blank is subjected to surface grinding and outer contour dimension processing to obtain the carbon ceramic brake disc.

7. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: In step 1, the carbon fiber directions of the upper and lower layers of carbon fiber unidirectional cloth of each layer of chopped carbon fiber layer form an angle of 90°.

8. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: The chemical vapor deposition conditions in step 1 are: methane flow rate is 80-180 L / h, nitrogen flow rate is 3-20 L / h, deposition temperature is 950-1100° C., and deposition time is 80-200 h.

9. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: In step 3, the impregnation liquid is a 30-50wt% phenolic resin alcohol solution.

10. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: In step 5, the temperature of the hot press is 150° C., the pressure is 3-10 MPa, and the hot pressing time is 4 hours.

11. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: The carbonization temperature in step 6 is 1000°C.

12. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: In step 8, pure silicon powder 1.1 times the mass of the brake disc blank is placed in the boron nitride crucible in advance.

13. The method for preparing a high-strength and high-toughness carbon ceramic brake disc according to claim 6, characterized in that: In step 8, the siliconizing treatment temperature is 1600-1700°C, the holding time is 2-4h, and the furnace pressure is less than 1000Pa.

Citation Information

Patent Citations

  • Method for preparing automobile brake disc from short fibers by compression molding

    CN108658613A

  • Preparation method of carbon-ceramic brake disc

    CN110483086A

  • Preparation method of carbon / ceramic brake disc with pure ceramic layer on surface

    CN110606763A

  • Preparation method of carbon fiber-reinforced silicon carbide brake disc

    CN113548902A

  • Carbon-ceramic brake disc with multi-layer structure and preparation method of carbon-ceramic brake disc

    CN113847365A