A molybdenum oxide target material and preparation method thereof
Through the multi-temperature zone reduction treatment of ammonium molybdate and static pressure sintering process, high-density oxidized molybdenum targets were prepared, which solved the adhesion and uniformity of existing molybdenum targets in magnetron sputtering coatings, and achieved the High efficiency and stable coating performance.
Patent Information
- Application Number
- CN202410126589.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-01-30
AI Technical Summary
The existing molybdenum oxide targets have problems such as adhesion, poor uniformity, difficult control and abnormal discharge during magnetron sputtering coating. In addition, high-purity and high-density oxidized molybdenum targets are subject to surface volatility in the treatment of oxygen supplementation in air atmosphere. , resulting in high conductivity, low coating efficiency and poor stability.
Using ammonium molybdate as raw material, the non-stoichiometric component molybdenum oxide powder is prepared through multi-temperature zone reduction treatment and mixed reduction atmosphere, and combined with cold isostatic molding and hot isostatic sintering technology to prepare high density, Magnesium oxide target material with uniform grain size.
The uniformity of the component, high density and low resistivity of the oxidized molybdenum target material is achieved. It is suitable for magnetron sputtering coating, which improves the adhesion and uniformity of the coating, reduces the risk of abnormal discharge, and meets the needs of industrial production.
Smart Images

Figure CN118005395B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sputtering target materials, and in particular to a molybdenum oxide target material and a preparation method thereof. Background Art
[0002] Molybdenum oxide film has some special optical properties, so it is particularly suitable for layer structures in optical and optoelectronic applications. It has the characteristics of diverse chemical composition and crystal phase structure, and its conductivity can be greatly adjusted. It has great application value in the fields of sensors, thin-film solar cells, photochromism, supercapacitors, OLED displays, etc. At present, there are many methods for preparing molybdenum oxide film, including hydrothermal synthesis, DC magnetron sputtering, vacuum evaporation, chemical vapor deposition, etc. The vacuum evaporation method mainly uses powder as the evaporation raw material for preparing tantalum oxide film. The prepared film is seriously affected by the particle size, morphology, looseness ratio, etc. of the powder. The adhesion and uniformity of the prepared film are poor, and the performance of the film cannot be guaranteed. Magnetron sputtering mostly uses reactive magnetron sputtering to prepare tantalum oxide film, that is, high-purity molybdenum target material is used as the sputtering source, and the sputtering film is adjusted by controlling process parameters such as vacuum degree and oxygen flow rate. The whole process is difficult to control, and it is easy to have abnormal discharge, target poisoning and other undesirable phenomena. If high-purity and high-density molybdenum oxide target is used for magnetron sputtering to prepare film layers, the above problems will be effectively solved. Therefore, the development and preparation of molybdenum oxide target materials suitable for magnetron sputtering coating has become an important issue that needs to be solved urgently and has far-reaching significance.
[0003] Chinese invention patent CN112359336A discloses a method for preparing a high-purity, high-density molybdenum trioxide target, comprising the following steps: obtaining high-purity molybdenum trioxide powder by roasting ammonium molybdate raw material, then hot pressing and sintering the powder to obtain a dense molybdenum trioxide blank, then oxygenating the molybdenum trioxide blank in an air atmosphere muffle furnace, and finally mechanically processing to obtain a molybdenum trioxide target. The preparation method performs oxygenation treatment in the air. Since the target material has been sintered densely, it is difficult for the gas to diffuse into the interior of the target material, resulting in differences in the uniformity of the target material inside and outside. And since molybdenum oxide has a low melting point and is very easy to volatilize above 600°C, there is a risk of surface volatilization when the target material is oxygenated in an air atmosphere.
[0004] Chinese invention patent CN 112359333A discloses a method for preparing a large-size, high-purity, high-density molybdenum trioxide target material, comprising the following steps: step 1, roasting ammonium molybdate to obtain high-purity molybdenum trioxide powder; step 2, ball milling the high-purity molybdenum trioxide powder; step 3, adding a certain amount of molding agent to the molybdenum trioxide powder after ball milling, and mixing evenly; step 4, pressing the mixed molybdenum trioxide powder into a blank; step 5, drying the molybdenum trioxide blank, placing it in a package, vacuuming and welding, and then hot isostatic pressing, removing the package to obtain a crude molybdenum trioxide target material; step 6, machining and cleaning the obtained crude molybdenum trioxide target material, and finally obtaining a high-purity and high-density molybdenum trioxide target material. The molybdenum trioxide target material prepared by the preparation method has a high conductivity, and can only be plated with a radio frequency power supply during magnetron sputtering coating, and the coating efficiency is low and the stability is poor, and it cannot be directly applied to industrial production. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the shortcomings of the prior art, the present invention provides a molybdenum oxide target material and a preparation method. The purpose of the invention is to obtain a molybdenum oxide sputtering target material with high density, uniform grain size and certain conductivity, which can be suitable for the needs of magnetron sputtering DC power supply equipment and is more conducive to meeting the practical application of magnetron sputtering in preparing molybdenum oxide film layers.
[0007] (II) Technical solution
[0008] To achieve the above object, the present invention provides the following technical solution: a method for preparing a molybdenum oxide target, the method for preparing the molybdenum oxide target comprising the following steps:
[0009] (1) subjecting 40-60 parts by weight of ammonium molybdate to a multi-temperature reduction treatment under a reducing atmosphere to obtain a high-purity molybdenum oxide powder;
[0010] (2) sieving 40-50 parts by weight of high-purity molybdenum oxide powder and pressing to obtain a pressed blank;
[0011] (3) hot isostatic pressing and sintering 30-50 parts by weight of the pressed blank to obtain a sintered molybdenum oxide target blank;
[0012] (4) Mechanically process 20-40 parts by weight of the sintered blank to obtain the desired molybdenum oxide target.
[0013] Preferably, the ammonium molybdate powder in (1) is one or a mixture of ammonium dimolybdate, ammonium tetramolybdate, ammonium heptamolybdate, ammonium octamolybdate and ammonium dodecomolybdate.
[0014] Preferably, the reducing atmosphere in (1) is a mixed gas of hydrogen and nitrogen, wherein the hydrogen content is 70-90 mol% and the nitrogen content is 10-30 mol%.
[0015] Preferably, the multi-temperature zone reduction treatment process in (1) is as follows: the reduction furnace is sequentially provided with three temperature zones from low temperature to high temperature, the ammonium molybdate powder passes through each temperature zone sequentially and is kept warm for a certain period of time, and the flow rate of the reducing atmosphere in the whole process is 15-25m 3 / h, and finally the required molybdenum oxide powder is obtained; the temperatures of the three temperature zones are respectively 250-350℃ for the low temperature zone, 350-500℃ for the medium temperature zone, and 500-650℃ for the high temperature zone; the insulation time of each temperature zone is respectively: 30-80min for the low temperature zone, 60-120min for the medium temperature zone, and 60-180min for the high temperature zone.
[0016] Preferably, the chemical composition of the molybdenum oxide powder in (1) is MoOx (2<x<3).
[0017] Preferably, the compression molding in (2) is to load the molybdenum oxide powder into a rubber mold, and then seal and fix it with a steel fixture and place it in a cold isostatic press for compression molding.
[0018] Preferably, the cold isostatic pressing process is: first increase the pressure to 100-120 MPa at a pressure increasing rate of 3-5 MPa / min, hold the pressure for 2-5 min, then increase the pressure to 200-240 MPa at a pressure increasing rate of 5-8 MPa / min, and hold the pressure for 10-20 min.
[0019] Preferably, the hot isostatic pressing sintering in (3) is to place the pressed blank obtained in step (2) into a bag for degassing, then vacuum seal it, and finally perform hot isostatic pressing sintering; the sintering temperature is 550-750°C, the pressure is 100-200Mpa, and the holding time is 2-4h.
[0020] Preferably, the density of the molybdenum oxide target blank in (3) is ≥98.5%, and the resistivity is ≤2x10 -3 Ωm.
[0021] Preferably, the mechanical processing in (4) includes cutting, and the cutting is performed using a diamond wire cutting device, and the surface after cutting is ground and polished.
[0022] (III) Beneficial technical effects
[0023] The present invention uses ammonium molybdate as a raw material, and adopts a process method of zone temperature control and mixed reducing atmosphere to prepare non-stoichiometric molybdenum oxide powder, which cannot be achieved by other methods. The zone control in the process ensures the full decomposition and exhaust of ammonium molybdate, and at the same time, under the action of the mixed reducing atmosphere, the growth rate of the crystal nucleus, the components of the powder and the particle size of the powder are effectively controlled. The molybdenum oxide powder finally obtained has uniform particle size and consistent composition, and is suitable for the preparation of molybdenum oxide target materials.
[0024] The present invention adopts ammonium molybdate as raw material to prepare non-stoichiometric molybdenum oxide powder, and then uses cold isostatic pressing and hot isostatic pressing sintering process to perform densification sintering. The molybdenum oxide target material finally obtained has uniform components, a density of ≥98.5%, and a resistivity of less than 2x10 -3 Ωm, which can realize the wide application of magnetron sputtering coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a flow chart for the preparation of molybdenum oxide target. DETAILED DESCRIPTION
[0026] Example 1
[0027] (1) 40 parts by weight of ammonium molybdate is subjected to a multi-temperature zone reduction treatment in a reducing atmosphere; the reducing atmosphere is a mixture of hydrogen and nitrogen, wherein the hydrogen content is 70 mol% and the nitrogen content is 10 mol%; the multi-temperature zone reduction treatment process is as follows: a reduction furnace is set up with three temperature zones from low temperature to high temperature in sequence, and the ammonium molybdate powder passes through each temperature zone in sequence and is kept warm for a certain period of time. The flow rate of the reducing atmosphere in the whole process is 15m 3 / h, and finally obtain the desired molybdenum oxide powder; the temperatures of the three temperature zones are respectively 250°C for the low temperature zone, 350°C for the medium temperature zone, and 500°C for the high temperature zone; the insulation time of each temperature zone is respectively: 30min for the low temperature zone, 60min for the medium temperature zone, and 60min for the high temperature zone; a mixture of ammonium dimolybdate and ammonium heptamolybdate is obtained, and the chemical composition of the mixture of ammonium dimolybdate and ammonium heptamolybdate is MoOx (2<x<3);
[0028] (2) 40 parts by weight of a mixture of ammonium dimolybdate and ammonium heptamolybdate are sieved and pressed into shape. The pressing is performed by loading the mixture of ammonium dimolybdate and ammonium heptamolybdate into a rubber mold, encapsulating and fixing the mixture with a steel fixture, and placing the mixture into a cold isostatic press for pressing. The pressure is first increased to 100 MPa at a pressure increase rate of 3 MPa / min, and the pressure is maintained for 2 minutes. The pressure is then increased to 200 MPa at a pressure increase rate of 5 MPa / min, and the pressure is maintained for 10 minutes to obtain a pressed blank.
[0029] (3) 30 parts by weight of the pressed blanks are subjected to hot isostatic pressing sintering. The hot isostatic pressing sintering is to place the pressed blanks obtained in step (2) into a bag for degassing, then vacuum seal, and finally perform hot isostatic pressing sintering. The sintering temperature is 550° C., the pressure is 100 MPa, and the holding time is 2 h to obtain a molybdenum oxide target sintered blank. The density of the molybdenum oxide target blank is ≥98.9%, and the resistivity is ≤2x10 -4 Ωm;
[0030] (4) 20 parts by weight of the sintered blank are subjected to mechanical processing, wherein the mechanical processing includes cutting using a diamond wire cutting device, and the surface after cutting is ground and polished to obtain the desired molybdenum oxide target.
[0031] Example 2
[0032] (1) 60 parts by weight of ammonium molybdate is subjected to multi-temperature zone reduction treatment under a reducing atmosphere; the reducing atmosphere is a mixture of hydrogen and nitrogen, wherein the hydrogen content is 90 mol% and the nitrogen content is 30 mol%; the multi-temperature zone reduction treatment process is as follows: a reduction furnace is set with three temperature zones from low temperature to high temperature in sequence, and the ammonium molybdate powder passes through each temperature zone in sequence and is kept warm for a certain period of time. The flow rate of the reducing atmosphere in the whole process is 25 m / s. 3 / h, and finally the desired molybdenum oxide powder is obtained; the temperatures of the three temperature zones are 350°C for the low temperature zone, 500°C for the medium temperature zone, and 650°C for the high temperature zone; the insulation time of each temperature zone is 80min for the low temperature zone, 120min for the medium temperature zone, and 180min for the high temperature zone; a mixture of ammonium dimolybdate and ammonium tetramolybdate is obtained, and the chemical composition of the mixture of ammonium dimolybdate and ammonium tetramolybdate is MoOx (2<x<3);
[0033] (2) sieving 50 parts by weight of a mixture of ammonium dimolybdate and ammonium tetramolybdate and pressing to form a rubber mold, encapsulating and fixing the mixture with a steel fixture and placing it in a cold isostatic press for pressing, first increasing the pressure to 120 MPa at a rate of 5 MPa / min, holding the pressure for 5 min, and then increasing the pressure to 240 MPa at a rate of 8 MPa / min, holding the pressure for 20 min, to obtain a pressed blank;
[0034] (3) 50 parts by weight of the pressed blanks are subjected to hot isostatic pressing sintering. The hot isostatic pressing sintering is to place the pressed blanks obtained in step (2) into a bag for degassing, then vacuum seal, and finally perform hot isostatic pressing sintering. The sintering temperature is 750° C., the pressure is 200 MPa, and the holding time is 4 h to obtain a molybdenum oxide target sintered blank. The molybdenum oxide target blank has a density of ≥99% and a resistivity of ≤5x10 -4 Ωm;
[0035] (4) 40 parts by weight of the sintered blank are subjected to mechanical processing, wherein the mechanical processing includes cutting using a diamond wire cutting device, and the surface after cutting is ground and polished to obtain the desired molybdenum oxide target.
[0036] Example 3
[0037] (1) 50 parts by weight of ammonium molybdate is subjected to a multi-temperature zone reduction treatment in a reducing atmosphere; the reducing atmosphere is a mixed gas of hydrogen and nitrogen, wherein the hydrogen content is 80 mol% and the nitrogen content is 20 mol%; the multi-temperature zone reduction treatment process is as follows: a reduction furnace is set up with three temperature zones from low temperature to high temperature in sequence, and the ammonium molybdate powder passes through each temperature zone in sequence and is kept warm for a certain period of time. The flow rate of the reducing atmosphere in the whole process is 20m 3 / h, and finally the desired molybdenum oxide powder is obtained; the temperatures of the three temperature zones are 300°C for the low temperature zone, 425°C for the medium temperature zone, and 600°C for the high temperature zone; the insulation time of each temperature zone is 55min for the low temperature zone, 90min for the medium temperature zone, and 120min for the high temperature zone; a mixture of ammonium heptamolybdate and ammonium octamolybdate is obtained, and the chemical composition of the mixture of ammonium heptamolybdate and ammonium octamolybdate is MoOx (2<x<3);
[0038] (2) 45 parts by weight of a mixture of ammonium heptamolybdate and ammonium octamolybdate are sieved and pressed into shape. The pressing is performed by placing the mixture of ammonium heptamolybdate and ammonium octamolybdate into a rubber mold, encapsulating and fixing the mixture with a steel fixture, and placing the mixture into a cold isostatic press for pressing. The pressure is first increased to 110 MPa at a pressure increasing rate of 4 MPa / min, and the pressure is maintained for 3.5 min. The pressure is then increased to 220 MPa at a pressure increasing rate of 6.5 MPa / min, and the pressure is maintained for 15 min to obtain a pressed blank.
[0039] (3) 40 parts by weight of the pressed blanks are subjected to hot isostatic pressing sintering. The hot isostatic pressing sintering is to place the pressed blanks obtained in step (2) into a bag for degassing, then vacuum seal, and finally perform hot isostatic pressing sintering. The sintering temperature is 650° C., the pressure is 150 MPa, and the holding time is 3 h to obtain a sintered molybdenum oxide target blank. The density of the molybdenum oxide target blank is ≥99%, and the resistivity is ≤3.5x10 -4 Ωm;
[0040] (4) 30 parts by weight of the sintered blank are subjected to mechanical processing, wherein the mechanical processing includes cutting using a diamond wire cutting device, and the surface after cutting is ground and polished to obtain the desired molybdenum oxide target.
[0041] Example 4
[0042] (1) 40 parts by weight of ammonium molybdate is subjected to a multi-temperature zone reduction treatment in a reducing atmosphere; the reducing atmosphere is a mixture of hydrogen and nitrogen, wherein the hydrogen content is 70 mol% and the nitrogen content is 10 mol%; the multi-temperature zone reduction treatment process is as follows: a reduction furnace is set up with three temperature zones from low temperature to high temperature in sequence, and the ammonium molybdate powder passes through each temperature zone in sequence and is kept warm for a certain period of time. The flow rate of the reducing atmosphere in the whole process is 15m 3 / h, and finally obtain the desired molybdenum oxide powder; the temperatures of the three temperature zones are respectively 250°C for the low temperature zone, 350°C for the medium temperature zone, and 500°C for the high temperature zone; the insulation time of each temperature zone is respectively: 30min for the low temperature zone, 60min for the medium temperature zone, and 60min for the high temperature zone; a mixture of ammonium dimolybdate and ammonium heptamolybdate is obtained, and the chemical composition of the mixture of ammonium dimolybdate and ammonium heptamolybdate is MoOx (2<x<3);
[0043] (2) sieving 50 parts by weight of a mixture of ammonium dimolybdate and ammonium tetramolybdate and pressing to form a rubber mold, encapsulating and fixing the mixture with a steel fixture and placing it in a cold isostatic press for pressing, first increasing the pressure to 120 MPa at a rate of 5 MPa / min, holding the pressure for 5 min, and then increasing the pressure to 240 MPa at a rate of 8 MPa / min, holding the pressure for 20 min, to obtain a pressed blank;
[0044] (3) 50 parts by weight of the pressed blanks are subjected to hot isostatic pressing sintering. The hot isostatic pressing sintering is to place the pressed blanks obtained in step (2) into a bag for degassing, then vacuum seal, and finally perform hot isostatic pressing sintering. The sintering temperature is 750° C., the pressure is 200 MPa, and the holding time is 4 hours to obtain a molybdenum oxide target sintered blank. The molybdenum oxide target blank has a density of ≥98.7% and a resistivity of ≤6x10 -4 Ωm;
[0045] (4) 30 parts by weight of the sintered blank are subjected to mechanical processing, wherein the mechanical processing includes cutting using a diamond wire cutting device, and the surface after cutting is ground and polished to obtain the desired molybdenum oxide target.
[0046] Example 5
[0047] (1) 60 parts by weight of ammonium molybdate is subjected to multi-temperature zone reduction treatment under a reducing atmosphere; the reducing atmosphere is a mixture of hydrogen and nitrogen, wherein the hydrogen content is 90 mol% and the nitrogen content is 30 mol%; the multi-temperature zone reduction treatment process is as follows: a reduction furnace is set with three temperature zones from low temperature to high temperature in sequence, and the ammonium molybdate powder passes through each temperature zone in sequence and is kept warm for a certain period of time. The flow rate of the reducing atmosphere in the whole process is 25 m / s. 3 / h, and finally the desired molybdenum oxide powder is obtained; the temperatures of the three temperature zones are 350°C for the low temperature zone, 500°C for the medium temperature zone, and 650°C for the high temperature zone; the insulation time of each temperature zone is 80min for the low temperature zone, 120min for the medium temperature zone, and 180min for the high temperature zone; a mixture of ammonium dimolybdate and ammonium tetramolybdate is obtained, and the chemical composition of the mixture of ammonium dimolybdate and ammonium tetramolybdate is MoOx (2<x<3);
[0048] (2) 45 parts by weight of a mixture of ammonium heptamolybdate and ammonium octamolybdate are sieved and pressed into shape. The pressing is performed by placing the mixture of ammonium heptamolybdate and ammonium octamolybdate into a rubber mold, encapsulating and fixing the mixture with a steel fixture, and placing the mixture into a cold isostatic press for pressing. The pressure is first increased to 110 MPa at a pressure increasing rate of 4 MPa / min, and the pressure is maintained for 3.5 min. The pressure is then increased to 220 MPa at a pressure increasing rate of 6.5 MPa / min, and the pressure is maintained for 15 min to obtain a pressed blank.
[0049] (3) 40 parts by weight of the pressed blanks are subjected to hot isostatic pressing sintering. The hot isostatic pressing sintering is to place the pressed blanks obtained in step (2) into a bag for degassing, then vacuum seal, and finally perform hot isostatic pressing sintering. The sintering temperature is 650° C., the pressure is 150 MPa, and the holding time is 3 h to obtain a molybdenum oxide target sintered blank. The molybdenum oxide target blank has a density of ≥98.5% and a resistivity of ≤2x10 -3 Ωm;
[0050] (4) 20 parts by weight of the sintered blank are subjected to mechanical processing, wherein the mechanical processing includes cutting using a diamond wire cutting device, and the surface after cutting is ground and polished to obtain the desired molybdenum oxide target.
[0051] Comparative Example 1
[0052] (1) 60 parts by weight of ammonium molybdate is subjected to reduction treatment in a reducing atmosphere; the reducing atmosphere is a mixed gas of hydrogen and nitrogen, wherein the hydrogen content is 90 mol % and the nitrogen content is 30 mol %; the multi-temperature zone reduction treatment process is as follows: a mixture of ammonium dimolybdate and ammonium tetramolybdate is obtained, and the chemical composition of the mixture of ammonium dimolybdate and ammonium tetramolybdate is MoOx (2<x<3);
[0053] (2) 45 parts by weight of a mixture of ammonium heptamolybdate and ammonium octamolybdate are sieved and pressed into shape. The pressing is performed by placing the mixture of ammonium heptamolybdate and ammonium octamolybdate into a rubber mold, encapsulating and fixing the mixture with a steel fixture, and placing the mixture into a cold isostatic press for pressing. The pressure is first increased to 110 MPa at a pressure increasing rate of 4 MPa / min, and the pressure is maintained for 3.5 min. The pressure is then increased to 220 MPa at a pressure increasing rate of 6.5 MPa / min, and the pressure is maintained for 15 min to obtain a pressed blank.
[0054] (3) Sintering 40 parts by weight of the pressed blank to obtain a sintered molybdenum oxide target blank, wherein the density of the molybdenum oxide target blank is ≥92.5% and the resistivity is ≤1x10 -3 Ωm;
[0055] (4) 20 parts by weight of the sintered blank are subjected to mechanical processing, wherein the mechanical processing includes cutting using a diamond wire cutting device, and the surface after cutting is ground and polished to obtain the desired molybdenum oxide target.
[0056] The performance test of the molybdenum oxide target prepared by the present invention is shown in Table 1.
[0057] Table 1: Target material performance index test.
[0058] project Density(%) Resistivity(Ωm) Example 1 98.9% <![CDATA[2x10 -4 ]]> Example 2 99% <![CDATA[5x10 -4 ]]> Example 3 99% <![CDATA[3.5x10 -4 ]]> Example 4 98.7% <![CDATA[6x10 -4 ]]> Example 5 98.5 <![CDATA[2x10 -3 ]]> Comparative Example 1 92.4 <![CDATA[1x10 -3 ]]>
[0059] It can be seen from Table 1 that the molybdenum oxide target material prepared by the present invention has uniform grain size and a resistivity of less than 2x10 -3 Ωm, its density is ≥98.5%, and all performance indicators meet the technical standards of high-quality target materials.
[0060] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing a molybdenum oxide target, characterized in that: The preparation method of the molybdenum oxide target comprises the following steps: (1) subjecting 40-60 parts by weight of ammonium molybdate to a multi-temperature reduction treatment in a reducing atmosphere to obtain high-purity molybdenum oxide powder; (2) sieving 40-50 parts by weight of high-purity molybdenum oxide powder and pressing it into a compact; (3) hot isostatic pressing and sintering 30-50 parts by weight of the pressed blank to obtain a sintered molybdenum oxide target blank; (4) Mechanically processing 20-40 parts by weight of the sintered blank to obtain the desired molybdenum oxide target; In the step (1), the ammonium molybdate is one or a mixture of ammonium dimolybdate, ammonium tetramolybdate, ammonium heptamolybdate, ammonium octamolybdate, and ammonium dodecomolybdate; In step (1), the reducing atmosphere is a mixed gas of hydrogen and nitrogen, wherein the hydrogen content is 70-90 mol% and the nitrogen content is 10-30 mol%; The multi-temperature zone reduction treatment process in step (1) is as follows: the reduction furnace is sequentially set with three temperature zones from low temperature to high temperature, and the ammonium molybdate powder passes through each temperature zone in turn and is kept warm for a certain period of time. The flow rate of the reducing atmosphere in the whole process is 15-25m 3 / h, and finally the required molybdenum oxide powder is obtained; the temperatures of the three temperature zones are 250-350℃ for the low temperature zone, 350-500℃ for the medium temperature zone, and 500-650℃ for the high temperature zone; the insulation time of each temperature zone is 30-80min for the low temperature zone, 60-120min for the medium temperature zone, and 60-180min for the high temperature zone; The pressing and molding in step (2) is to load the molybdenum oxide powder into a rubber mold, and then use a steel fixture to seal and fix it into a cold isostatic press for pressing and molding; The cold isostatic pressing process is as follows: first, the pressure is increased to 100-120 MPa at a pressure increasing rate of 3-5 MPa / min, and the pressure is maintained for 2-5 minutes, and then the pressure is increased to 200-240 MPa at a pressure increasing rate of 5-8 MPa / min, and the pressure is maintained for 10-20 minutes; The hot isostatic pressing sintering in step (3) is to place the pressed blank obtained in step (2) into a bag for degassing, then vacuum seal it, and finally perform hot isostatic pressing sintering; the sintering temperature is 550-750°C, the pressure is 100-200Mpa, and the holding time is 2-4h.
2. The method for preparing a molybdenum oxide target according to claim 1, characterized in that: The chemical composition of the molybdenum oxide powder in (1) is MoOx, and the range of x is 2<x<3.
3. The method for preparing a molybdenum oxide target according to claim 1, characterized in that: The density of the sintered molybdenum oxide target in (3) is ≥98.5%, and the resistivity is ≤2x10 -3 Ωm.
4. The method for preparing a molybdenum oxide target according to claim 1, characterized in that: The mechanical processing in (4) includes cutting, which is performed using a diamond wire cutting device, and the surface after cutting is ground and polished.