A high temperature resistant stainless steel welded pipe and its preparation process

By combining metal oxide powders such as magnesium oxide and nickel oxide with aluminum powder and carbon nanotubes, spraying ceramic coatings, and using fluorinated nanosilicon dioxide hydrophobic coatings, the corrosion problem of stainless steel welded pipes under high temperature and high humidity conditions is solved. , significantly improves its corrosion resistance and high temperature resistance.

CN118007131BActive Publication Date: 2024-11-26JIANG SU BAN DE RUI BU XIU GANG GUAN YE YOU XIAN GONG SI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410191408.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-21
Publication Date
2024-11-26
Estimated Expiration
2044-02-21

AI Technical Summary

Technical Problem

Stainless steel welded pipes are prone to corrosion under high temperature and high humidity conditions. The adhesion of existing anticorrosion coatings decreases under the action of moisture penetration, resulting in the coating falling off and unable to meet the long-term corrosion resistance requirements.

Method used

Magnesium oxide, nickel oxide, yttrium oxide, aluminum oxide, zinc oxide powder and zirconium oxide milling balls are used to prepare ceramic powder, and combine it with aluminum powder, carbon nanotubes, polyvinyl alcohol, boric acid, etc. through atmospheric plasma spraying system Spray the ceramic coating and subsequently enhance surface protection using fluorinated nanosilicon dioxide hydrophobic coating.

Benefits of technology

It improves the corrosion resistance and high temperature resistance of stainless steel welded pipes, enhances the hardness of ceramic coatings, reduces moisture corrosion by hydrophobic coatings, and increases the coating strength and adhesion of carbon nanotubes, meeting the long-term use requirements in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118007131B_ABST
    Figure CN118007131B_ABST
Patent Text Reader

Abstract

The invention discloses a high-temperature resistant stainless steel welded pipe and a preparation process thereof, belonging to the technical field of stainless steel welded pipes. An atmospheric plasma spraying system is adopted to spray composite powder on the surface of the stainless steel welded pipe after sandblasting and cleaning, and then the pipe is transferred to an annealing furnace for heat preservation treatment under oxygen conditions to obtain the stainless steel welded pipe with a ceramic coating. A spray gun is used to spray a hydrophobic coating on the surface of the stainless steel welded pipe with the ceramic coating, and the pipe is dried to obtain the high-temperature resistant stainless steel welded pipe. The use of a variety of metal oxides as raw materials is helpful to improve the entropy value of the metal oxide powder, and is helpful to improve the hardness and high-temperature resistance of the ceramic coating. The hydrophobic coating is helpful to reduce the erosion of the high-temperature resistant stainless steel welded pipe by water. The part of the carbon nanotube located on the surface of the coating reacts with oxygen to form uniform pores to release thermal stress, further increase the high-temperature resistance of the ceramic coating, and at the same time, help to increase the specific surface area and roughness of the ceramic coating, and increase the adhesion of the hydrophobic coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel welded pipes, and in particular relates to a high temperature resistant stainless steel welded pipe and a preparation process thereof. Background Art

[0002] Stainless steel welded pipe is a steel pipe made by welding common steel or steel strip after curling and forming by a unit and a die. The production process of stainless steel welded pipe is simple, the production efficiency is high, the varieties and specifications are many, and the equipment investment is small, but the general strength is lower than that of seamless steel pipe. However, with the rapid development of high-quality strip steel continuous rolling production and the advancement of welding and inspection technology, the quality of welds is constantly improving, the varieties and specifications of welded steel pipes are increasing, and they have replaced seamless steel pipes in more and more fields, especially in heat exchange equipment pipes, decorative pipes, medium and low pressure fluid pipes, etc.

[0003] There are many types of stainless steel welded pipes according to material classification. Different types of stainless steel welded pipes have different performances, so they need to be selected. In some scenarios where stainless steel welded pipes are widely used, such as boiler rooms in power stations, using all alloys with high content of precious metals such as nickel will undoubtedly increase the project cost, so some lower-priced stainless steel will be used appropriately. However, under extreme conditions such as high temperature and high humidity, stainless steel welded pipes will also be corroded, and the subsequent maintenance costs will also increase.

[0004] In order to increase the corrosion resistance of ordinary stainless steel welded pipes, surface treatment is generally required. The Chinese patent with announcement number CN115368786B uses the method of spraying heat-resistant anti-corrosion coating to prepare high-temperature resistant and corrosion-resistant stainless steel welded pipes, which makes up for the problem that the existing super austenitic stainless steel welded pipes are easily oxidized under high temperature conditions. However, under high humidity conditions, the penetration of water will cause the adhesion of the anti-corrosion coating to decrease, resulting in the problem of coating shedding, which is not conducive to the long-term corrosion resistance requirements of stainless steel welded pipes under special applications. Summary of the invention

[0005] One of the purposes of the present invention is to provide a high temperature resistant stainless steel welded pipe to solve the problem; the second purpose is to provide a preparation process of the high temperature resistant stainless steel welded pipe.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A preparation process of a high temperature resistant stainless steel welded pipe comprises the following steps:

[0008] Step 1: Mix magnesium oxide powder, nickel oxide powder, yttrium oxide powder, aluminum oxide powder and zinc oxide powder and transfer them to a ball mill, then add zirconium oxide grinding balls with a diameter of 5-10 mm, add deionized water, and ball mill for 20-24 hours at 300-400r / min. After discharging, dry at 50-70°C for 6-8 hours, and pass through an 80-mesh sieve to obtain a mixed powder; pour the mixed powder into a mold for compression molding, transfer the green body to a muffle furnace after demolding, heat it to 900-1000°C at a rate of 3-5°C / min, keep it warm for 10-12 hours, then cool it to 20-30°C at a rate of 20-40°C / s, crush, ball mill, and pass through a 400-500 mesh sieve to obtain an oxide ceramic powder;

[0009] Furthermore, the mass ratio of magnesium oxide powder, nickel oxide powder, yttrium oxide powder, aluminum oxide powder, zinc oxide powder, zirconium oxide grinding balls and deionized water is 1.6:1.6:1.6:1.6:1.6:1:4-5.5.

[0010] Step 2: Add oxide ceramic powder, aluminum powder, carbon nanotubes and deionized water into a ball mill, and mix them by ball milling at 200-400 r / min for 2-4 hours, then add polyvinyl alcohol and boric acid, and continue ball milling for 1-2 hours. After filtering the material, blow dry it, crush it, ball mill it, and pass it through a 400-500 mesh sieve to obtain a composite powder;

[0011] Furthermore, the mass ratio of oxide ceramic powder, aluminum powder, carbon nanotubes, deionized water, polyvinyl alcohol and boric acid is 9:1.5-2:0.5-1:5-6:0.35-0.4:0.05-0.1.

[0012] Step 3: Use an atmospheric plasma spraying system to spray the composite powder on the surface of the stainless steel welded pipe after sandblasting and cleaning to obtain a coating with a thickness of 0.5-0.8 mm, and then transfer the coated stainless steel welded pipe to an annealing furnace, introduce oxygen at a rate of 1-1.5L / min, keep warm at 600-700℃ for 40-60min, and cool naturally to obtain a stainless steel welded pipe with a ceramic coating;

[0013] Step 4: Use cyclohexane to ultrasonically disperse the fluorinated nano-silica into a hydrophobic coating with a solid content of 30-35%, use a spray gun to spray the hydrophobic coating on the surface of the stainless steel welded pipe with a ceramic coating, and dry it to obtain a high-temperature resistant stainless steel welded pipe.

[0014] Furthermore, the spraying distance of the spray gun is 15-20 cm and the pressure is 0.1-0.12 MPa.

[0015] Further, the fluorinated nano-silicon dioxide is prepared by the following steps:

[0016] Ammonia water with a mass fraction of 5-10%, ethanol aqueous solution with a mass fraction of 85-90% and tetraethoxysilane are added into a reaction kettle, stirred for 10-12 hours at 200-500r / min, filtered and dried to obtain nano silicon dioxide powder; nano silicon dioxide powder, perfluoroalkyl triethoxysilane and anhydrous ethanol are stirred and mixed, ultrasonically dispersed for 2-4 hours, filtered and dried to obtain fluorinated nano silicon dioxide.

[0017] Furthermore, the usage ratio of ammonia water, ethanol aqueous solution and tetraethoxysilane is 8-10 mL: 170-180 mL: 4-5 mL.

[0018] Furthermore, the usage ratio of nano silicon dioxide powder, perfluoroalkyltriethoxysilane and anhydrous ethanol is 1g:3g:30-40mL.

[0019] Beneficial effects of the present invention:

[0020] The high-temperature resistant stainless steel welded pipe of the present invention has a ceramic coating and a hydrophobic coating sequentially coated on the surface of the stainless steel welded pipe, which helps to improve the corrosion resistance of the stainless steel welded pipe.

[0021] When preparing metal oxide powder, magnesium oxide powder, nickel oxide powder, yttrium oxide powder, aluminum oxide powder and zinc oxide powder are selected and mixed. Using a variety of metal oxides as raw materials helps to increase the entropy value of the metal oxide powder, which helps to improve the hardness and high temperature resistance of the ceramic coating; the hydrophobic coating helps to reduce the erosion of water on high temperature resistant stainless steel welded pipes.

[0022] Atmospheric plasma spraying is helpful for preparing coatings efficiently and stably. The composite powder also contains aluminum powder, carbon nanotubes, polyvinyl alcohol and boric acid. The polyvinyl alcohol plays a finishing role, which helps to keep the particle size and shape of the composite powder uniform and facilitate spraying. The carbon nanotubes play a pinning role, which helps to increase the strength and thermal shock resistance of the ceramic coating. Under the high temperature of the annealing furnace, boric acid helps the aluminum powder to melt, further increasing the strength of the ceramic coating, and the part of the carbon nanotubes located on the surface of the coating reacts with oxygen to form uniform pores to release thermal stress, further increasing the high temperature resistance of the ceramic coating. At the same time, it helps to increase the specific surface area and roughness of the ceramic coating and increase the adhesion of the hydrophobic coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention will be further described below in conjunction with the accompanying drawings.

[0024] Figure 1 This is a surface micrograph of a stainless steel welded pipe with a ceramic coating according to Example 3 of the present invention;

[0025] Figure 2 This is a surface micrograph of the stainless steel welded pipe with ceramic coating in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Embodiment 1: This embodiment provides a high temperature resistant stainless steel welded pipe, comprising the following implementation steps:

[0028] Step 1: Mix 16kg of magnesium oxide powder, 16kg of nickel oxide powder, 16kg of yttrium oxide powder, 16kg of aluminum oxide powder and 16kg of zinc oxide powder and transfer them to a ball mill, then add 10kg of zirconium oxide grinding balls with a diameter of 5mm, add 40kg of deionized water, ball mill at 300r / min for 20h, dry at 50°C for 6h after discharging, and pass through an 80-mesh sieve to obtain a mixed powder; pour the mixed powder into a mold for compression molding, transfer the blank to a muffle furnace after demolding, heat it to 900°C at a rate of 3°C / min, keep it warm for 10h, then cool it to 20°C at a rate of 20°C / s, crush, ball mill, and pass through a 400-mesh sieve to obtain an oxide ceramic powder.

[0029] Step 2: Add 9kg oxide ceramic powder, 1.5kg aluminum powder, 0.5kg carbon nanotubes and 5kg deionized water into a ball mill, mix them at 200r / min for 2h, then add 0.35kg polyvinyl alcohol and 0.05kg boric acid, continue ball milling for 1h, filter the material, dry it with air, crush it, ball mill it, and pass it through a 400-mesh sieve to obtain a composite powder.

[0030] Step 3: Use an atmospheric plasma spraying system to spray the composite powder on the surface of the stainless steel welded pipe after sandblasting and cleaning to obtain a coating with a thickness of 0.5 mm, and then transfer the coated stainless steel welded pipe to an annealing furnace, introduce oxygen at a rate of 1 L / min, keep the temperature at 600 ° C for 40 minutes, and cool naturally to obtain a stainless steel welded pipe with a ceramic coating;

[0031] The working current of the atmospheric plasma spraying system is 550A, the voltage is 70V, the argon flow rate is 40L / min, the hydrogen flow rate is 10L / min, the composite powder flow rate is 30g / min, and the spraying distance is 10cm.

[0032] Step 4: Add 80L of 5% ammonia water, 1700L of 85% ethanol aqueous solution and 40L of tetraethoxysilane into the reaction kettle, stir for 10h at 200r / min, filter and dry to obtain nano-silica powder; stir and mix 100g of nano-silica powder, 300g of perfluoroalkyltriethoxysilane and 3L of anhydrous ethanol, ultrasonically disperse for 2h, filter and dry to obtain fluorinated nano-silica.

[0033] Step 5: Use cyclohexane to ultrasonically disperse the fluorinated nano-silica into a hydrophobic coating with a solid content of 30%, and use a spray gun to spray the hydrophobic coating on the surface of the stainless steel welded pipe with a ceramic coating. The spraying distance of the spray gun is 15 cm, the pressure is 0.1 MPa, and it is dried to obtain a high-temperature resistant stainless steel welded pipe.

[0034] Embodiment 2: This embodiment provides a high temperature resistant stainless steel welded pipe, comprising the following implementation steps:

[0035] Step 1: Mix 16kg of magnesium oxide powder, 16kg of nickel oxide powder, 16kg of yttrium oxide powder, 16kg of aluminum oxide powder and 16kg of zinc oxide powder and transfer them to a ball mill, then add 10kg of zirconia grinding balls with a diameter of 8mm, add 50kg of deionized water, ball mill at 350r / min for 22h, dry at 65°C for 7h after discharging, and pass through an 80-mesh sieve to obtain a mixed powder; pour the mixed powder into a mold for compression molding, transfer the blank to a muffle furnace after demolding, heat it to 950°C at a rate of 4°C / min, keep it warm for 11h, then cool it to 25°C at a rate of 30°C / s, crush, ball mill, and pass through a 450-mesh sieve to obtain an oxide ceramic powder.

[0036] Step 2: Add 9kg oxide ceramic powder, 1.8kg aluminum powder, 0.8kg carbon nanotubes and 5.5kg deionized water into a ball mill, and mix them by ball milling at 300r / min for 3h. Then add 0.38kg polyvinyl alcohol and 0.08kg boric acid, and continue ball milling for 1.5h. After filtering the material, dry it with air, crush it, ball mill it, and pass it through a 450-mesh sieve to obtain a composite powder.

[0037] Step 3: Use an atmospheric plasma spraying system to spray the composite powder on the surface of the stainless steel welded pipe after sandblasting and cleaning to obtain a coating with a thickness of 0.6 mm, and then transfer the coated stainless steel welded pipe to an annealing furnace, introduce oxygen at a rate of 1.2 L / min, keep warm at 650 ° C for 50 minutes, and cool naturally to obtain a stainless steel welded pipe with a ceramic coating;

[0038] The working current of the atmospheric plasma spraying system is 550A, the voltage is 70V, the argon flow rate is 40L / min, the hydrogen flow rate is 10L / min, the composite powder flow rate is 30g / min, and the spraying distance is 10cm.

[0039] Step 4: Add 90L of 8% ammonia water, 1750L of 88% ethanol aqueous solution and 45L of tetraethoxysilane into the reaction kettle, stir at 350r / min for 11h, filter and dry to obtain nano-silica powder; stir 100g of nano-silica powder, 300g of perfluoroalkyltriethoxysilane and 3.5L of anhydrous ethanol, mix and ultrasonically disperse for 3h, filter and dry to obtain fluorinated nano-silica.

[0040] Step 5: Use cyclohexane to ultrasonically disperse the fluorinated nano-silica into a hydrophobic coating with a solid content of 32%, and use a spray gun to spray the hydrophobic coating on the surface of the stainless steel welded pipe with a ceramic coating. The spraying distance of the spray gun is 18 cm, the pressure is 0.11 MPa, and it is dried to obtain a high-temperature resistant stainless steel welded pipe.

[0041] Embodiment 3 This embodiment provides a high temperature resistant stainless steel welded pipe, comprising the following implementation steps:

[0042] Step 1: Mix 16kg of magnesium oxide powder, 16kg of nickel oxide powder, 16kg of yttrium oxide powder, 16kg of aluminum oxide powder and 16kg of zinc oxide powder and transfer them to a ball mill, then add 10kg of zirconium oxide grinding balls with a diameter of 10mm, add 55kg of deionized water, ball mill at 400r / min for 24h, dry at 70°C for 8h after discharging, and pass through an 80-mesh sieve to obtain a mixed powder; pour the mixed powder into a mold for compression molding, transfer the blank to a muffle furnace after demolding, heat it to 1000°C at a rate of 5°C / min, keep it warm for 12h, then cool it to 30°C at a rate of 40°C / s, crush, ball mill, and pass through a 500-mesh sieve to obtain an oxide ceramic powder.

[0043] Step 2: Add 9kg of oxide ceramic powder, 2kg of aluminum powder, 1kg of carbon nanotubes and 6kg of deionized water into a ball mill, and mix them by ball milling at 400r / min for 4h. Then add 0.4kg of polyvinyl alcohol and 0.1kg of boric acid, and continue ball milling for 2h. After filtering the material, dry it with air, crush it, ball mill it, and pass it through a 500-mesh sieve to obtain a composite powder.

[0044] Step 3: Use an atmospheric plasma spraying system to spray the composite powder on the surface of the stainless steel welded pipe after sandblasting and cleaning to obtain a coating with a thickness of 0.8 mm. Then transfer the coated stainless steel welded pipe to an annealing furnace, introduce oxygen at a rate of 1.5 L / min, keep the temperature at 700°C for 60 minutes, and cool naturally to obtain a stainless steel welded pipe with a ceramic coating (see the enlarged view of its surface for details). Figure 1 );

[0045] The working current of the atmospheric plasma spraying system is 550A, the voltage is 70V, the argon flow rate is 40L / min, the hydrogen flow rate is 10L / min, the composite powder flow rate is 30g / min, and the spraying distance is 10cm.

[0046] Step 4: Add 100L of 10% ammonia water, 1800L of 90% ethanol aqueous solution and 50L of tetraethoxysilane into the reaction kettle, stir for 12h at 500r / min, filter and dry to obtain nano-silica powder; stir and mix 100g of nano-silica powder, 300g of perfluoroalkyltriethoxysilane and 4L of anhydrous ethanol, ultrasonically disperse for 4h, filter and dry to obtain fluorinated nano-silica.

[0047] Step 5: Use cyclohexane to ultrasonically disperse the fluorinated nano-silica into a hydrophobic coating with a solid content of 35%, and use a spray gun to spray the hydrophobic coating on the surface of the stainless steel welded pipe with a ceramic coating. The spraying distance of the spray gun is 20 cm, the pressure is 0.12 MPa, and it is dried to obtain a high-temperature resistant stainless steel welded pipe.

[0048] Comparative Example 1: Based on Example 3, no carbon nanotubes are added in step 2, and then a stainless steel welded pipe with a ceramic coating is prepared according to step 3 (the enlarged view of the surface is shown in FIG. Figure 2 ), and the other steps remain unchanged to prepare a high temperature resistant stainless steel welded pipe.

[0049] Comparative Example 2: Based on Example 3, directly according to step five, a spray gun is used to spray the hydrophobic coating on the surface of the stainless steel welded pipe after sandblasting and cleaning to prepare a high-temperature resistant stainless steel welded pipe.

[0050] The material of the stainless steel welded pipe in the embodiment and the comparative example is 317L austenitic stainless steel.

[0051] The performance tests of Examples 1 to 3 and Comparative Examples 1 to 2 were carried out according to GB / T2423.17-93. A YWX / Q-150 salt spray tester was used to prepare a 5wt% NaCl aqueous solution, adjust the pH to 7 as the solution used for the salt spray test spray, the temperature was 35°C, and the salt spray deposition was 2mL / 80cm 3h, the stainless steel welded pipe is 30° to the vertical direction, and the rust area ratio (%) of each group of stainless steel welded pipes is observed and calculated after 48 h; different stainless steel welded pipes are placed in a muffle furnace, kept at 500°C for 30 min, and then immersed in water at room temperature within 3 s, and thermal shock tests are carried out in turn, and the cycle is 100 times to observe the surface condition of the coating to see if there is peeling or other phenomena; stainless steel plates of the same specification and thickness of 10 mm are selected, and coatings are prepared according to the corresponding methods in the embodiments and comparative examples, and the hydrophobic angle is detected, and then the hydrophobic angle is detected again after the salt spray test ("\" indicates untested); the results are shown in Table 1:

[0052] Table 1

[0053]

[0054] It can be seen from Table 1 that the coatings in Examples 1 to 3 have good corrosion resistance under the neutral salt spray test, and no rust occurs. In addition, the surface ceramic coating remains intact after the thermal shock test, and has better high temperature resistance. The hydrophobic coating has a better adhesion effect on the surface of the ceramic coating.

[0055] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A preparation process for a high temperature resistant stainless steel welded pipe, characterized in that: The steps include: Step 1: Add oxide ceramic powder, aluminum powder, carbon nanotubes and deionized water into a ball mill, mix at 200-400 r / min for 2-4 hours, then add polyvinyl alcohol and boric acid and ball mill for 1-2 hours, filter the material, dry, crush, ball mill, and pass through a 400-500 mesh sieve to obtain a composite powder; Step 2: Use an atmospheric plasma spraying system to spray the composite powder on the surface of the stainless steel welded pipe after sandblasting and cleaning, then transfer it to an annealing furnace, introduce oxygen at a rate of 1-1.5L / min, keep it at 600-700℃ for 40-60min, and cool it naturally to obtain a stainless steel welded pipe with a ceramic coating; Step 4: Ultrasonic dispersion of fluorinated nano-silica into a hydrophobic coating with a solid content of 30-35% using cyclohexane, spraying the hydrophobic coating on the surface of the stainless steel welded pipe with a ceramic coating using a spray gun, and drying to obtain a high-temperature resistant stainless steel welded pipe; The raw materials of the oxide ceramic powder are selected from magnesium oxide powder, nickel oxide powder, yttrium oxide powder, aluminum oxide powder and zinc oxide powder; The mass ratio of the oxide ceramic powder, aluminum powder, carbon nanotubes, deionized water, polyvinyl alcohol and boric acid in step 1 is 9:1.5-2:0.5-1:5-6:0.35-0.4:0.05-0.1; The fluorinated nano-silicon dioxide is prepared by the following steps: Ammonia water with a mass fraction of 5-10%, ethanol aqueous solution with a mass fraction of 85-90% and tetraethoxysilane are added into a reaction kettle, stirred for 10-12 hours at 200-500 r / min, filtered and dried to obtain nano-silica powder, which is then stirred and mixed with perfluoroalkyltriethoxysilane and anhydrous ethanol, ultrasonically dispersed, filtered and dried to obtain fluorinated nano-silica.

2. The preparation process of a high temperature resistant stainless steel welded pipe according to claim 1, characterized in that: Step 2: The thickness of the composite powder sprayed is 0.5-0.8 mm.

3. The preparation process of a high temperature resistant stainless steel welded pipe according to claim 1, characterized in that: In step 3, the spraying distance of the spray gun is 15-20 cm, and the pressure is 0.1-0.12 MPa.

4. The preparation process of a high temperature resistant stainless steel welded pipe according to claim 1, characterized in that: The oxide ceramic powder is prepared by the following steps: Mix magnesium oxide powder, nickel oxide powder, yttrium oxide powder, aluminum oxide powder and zinc oxide powder and transfer them to a ball mill, add zirconium oxide grinding balls and deionized water, and ball mill at 300-400r / min for 20-24h, discharge, dry, and pass through an 80-mesh sieve to obtain a mixed powder, which is then compression molded and transferred to a muffle furnace, heated to 900-1000°C at a rate of 3-5°C / min, kept warm for 10-12h, then cooled to 20-30°C at a rate of 20-40°C / s, crushed, ball milled, and passed through a 400-500 mesh sieve to obtain an oxide ceramic powder.

5. The process for preparing a high temperature resistant stainless steel welded pipe according to claim 4, characterized in that: The mass ratio of the magnesium oxide powder, the nickel oxide powder, the yttrium oxide powder, the aluminum oxide powder, the zinc oxide powder, the zirconium oxide grinding balls and the deionized water is 1.6:1.6:1.6:1.6:1.6:1:4-5.

5.

6. The process for preparing a high temperature resistant stainless steel welded pipe according to claim 1, characterized in that: The dosage ratio of the ammonia water, the ethanol aqueous solution and tetraethoxysilane is 8-10 mL: 170-180 mL: 4-5 mL.

7. The process for preparing a high temperature resistant stainless steel welded pipe according to claim 1, characterized in that: The dosage ratio of the nano silicon dioxide powder, perfluoroalkyl triethoxysilane and anhydrous ethanol is 1g:3g:30-40mL.

8. A high temperature resistant stainless steel welded pipe, characterized in that: It is prepared by the preparation process described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • A manufacturing process for super austenitic high-temperature and corrosion-resistant stainless steel welded pipes

    CN115368786B

  • Preparation method of ceramic surface metal coating

    CN113493351A

  • Method of conductive inorganic carbon NANO composite powder

    KR1020120056075A

  • Ceramic composites electrode for electric discharge machining and manufacturing method thereof

    KR1020130043807A

  • Ceramic composite for plasma processing apparatus and manufacturing mehtod thereof

    KR1020180091560A