A method for preparing precursor for ultra-high performance carbon fiber
Through atom transfer radical polymerization and microfluidic spinning, the microporous defects and skin-core structure problems in the preparation of traditional PAN precursors were solved, and high-performance carbon fiber precursors were prepared, achieving the production of ultra-high-performance carbon fibers and improving Improve the mechanical and thermal stability properties of carbon fiber.
Patent Information
- Application Number
- CN202410267012.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-08
AI Technical Summary
There are microporous defects and skin-core structural problems in the traditional PAN precursor preparation process, which affect the mechanical properties, thermal stability and surface properties of carbon fibers, leading to performance degradation. Domestic ultra-high-performance carbon fibers such as T1000 and T1100 are difficult to achieve.
Atom transfer radical polymerization (ATRP) is used for precise synthesis of PAN polymer, combined with microfluidic spinning method, and ultra-high performance carbon fiber precursors with uniform structure and high stereoregularity are prepared by precisely controlling the spinning process.
The preparation of ultra-high-performance carbon fibers has been achieved. The produced raw fibers have a dense internal structure, smooth appearance, and significantly improved mechanical properties and thermal stability. The breaking strength and modulus of carbon fibers have reached high standards. The T1000 pass rate has reached more than 90%, and T1100 has passed the test. The rate exceeds 60%.
Smart Images

Figure CN118007284B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon fiber precursor preparation, and specifically relates to a method for preparing ultra-high performance carbon fiber precursor. Background Art
[0002] Carbon fiber is an advanced material with excellent properties such as high strength, high modulus, low density, high heat resistance, and high corrosion resistance. It is widely used in aerospace, national defense, automobile manufacturing, sports equipment and other fields. In particular, ultra-high performance carbon fiber has become an important industrial material for military aircraft and aerospace equipment. The preparation process of carbon fiber mainly includes the steps of precursor preparation, pre-oxidation, carbonization and graphitization. Among them, the preparation of precursor is the key link that affects the performance of carbon fiber. The molecular structure, molecular weight, molecular weight distribution, comonomer content, stereoregularity and other parameters of the precursor have an important influence on the mechanical properties, thermal stability, surface properties and the like of carbon fiber.
[0003] At present, the industry mainly uses polyacrylonitrile (PAN) as raw material to prepare carbon fiber. PAN is a linear polymer, which is copolymerized by acrylonitrile (AN) and a small amount of comonomers (such as itaconic acid, acrylic acid, etc.). The advantages of PAN are high carbon content, low oxygen content, high cyclization rate, good thermal stability, etc., which makes it suitable as a precursor of carbon fiber.
[0004] However, there are some technical problems in the traditional PAN precursor preparation process, which are mainly manifested in the following two aspects:
[0005] 1. Microporous defects of precursor fibers: During the preparation of PAN precursor fibers, due to factors such as the non-uniformity of the polymerization reaction, the instability of the solution, and the uncontrollability of the spinning process, some tiny gaps or holes will be generated in the precursor fibers, which are called microporous defects. These microporous defects will affect the mechanical properties, thermal stability, and surface properties of the precursor fibers, reduce the quality and uniformity of the precursor fibers, and also affect the subsequent pre-oxidation, carbonization, and graphitization processes, resulting in a decrease in the performance of the carbon fibers;
[0006] 2. The skin-core structure of the precursor: During the pre-oxidation of PAN precursor, due to the radial temperature gradient and oxygen concentration gradient of the precursor, the oxidation reaction rates of the surface and inner layers of the precursor are different, forming different degrees of cyclization and cross-linking, which leads to different structures and properties of the surface and inner layers of the precursor, which is called the skin-core structure. This skin-core structure will affect the mechanical properties, thermal stability and surface properties of the precursor, causing the radial shrinkage of the precursor and the collapse of the epidermis, reducing the quality and uniformity of the precursor, and will also affect the subsequent carbonization and graphitization process, resulting in a decrease in the performance of the carbon fiber.
[0007] my country began to study polyacrylonitrile carbon fiber and its application technology in the 1970s. After years of research, my country's carbon fiber industry has made some progress in key technologies, equipment, and industrial production; however, high-end carbon fiber has only reached the T700 and T800 levels, and ultra-high performance carbon fibers such as T1000 and T1100 are still blank in China due to process technology difficulties.
[0008] In order to solve these technical problems and improve the quality and performance of PAN precursor, the present invention proposes a method for preparing precursor for ultra-high performance carbon fiber by accurately synthesizing PAN polymer using atom transfer radical polymerization (ATRP) and spinning using microfluidic spinning. Summary of the invention
[0009] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for preparing ultra-high performance carbon fiber precursor. The ultra-high performance precursor produced by this method can produce ultra-high performance carbon fiber after carbonization, filling the gap in domestic ultra-high performance carbon fiber.
[0010] To achieve the above object, the technical solution adopted by the present invention is:
[0011] A method for preparing ultra-high performance carbon fiber precursor, comprising the following steps:
[0012] S1. Polymerization: Add redox initiator (R), copper salt and ligand to water containing acrylonitrile (AN) and comonomer (M) to form a heterogeneous reaction system for polymerization. After the reaction is completed, PAN polymer powder is obtained by filtering, washing and drying. The chemical reaction equation involved is as follows:
[0013]
[0014] S2, spinning solution preparation: dissolving the obtained PAN polymer powder in a solvent to prepare a spinning solution;
[0015] S3, spinning: the spinning solution is sent into the microfluidic chip through a precision metering pump, and then reaches the spinneret after passing through the filter, and a thin stream of the original solution is sprayed out, and after passing through a section of air layer, it enters the coagulation bath, and forms primary fibers in the coagulation bath;
[0016] S4. Drawing preparation: The obtained spun fibers are subjected to water washing, hot water drawing, oiling, drying, steam drawing and winding to obtain ultra-high performance carbon fiber precursor.
[0017] In this technical solution, atom transfer radical polymerization (ATRP) is a controllable / active radical polymerization method, which can achieve precise control of the molecular weight, molecular weight distribution, chain end, chain architecture and functionalization of the polymer, thereby obtaining PAN polymer powder with uniform structure and high stereoregularity; microfluidic spinning is a new technology that uses microfluidic chips for spinning, which can achieve precise control of the spinning process, thereby obtaining primary fibers with high orientation, high purity and gradient nanostructure.
[0018] In a preferred embodiment, the comonomer is itaconic acid, acrylic acid or its derivatives, and its content is 2-7% of the mass of PAN polymer. The mass ratio of acrylonitrile to the comonomer is 9-50:1. The redox initiator is azobisisobutyronitrile. The copper salt and the ligand are CuBr2 and TPMA, and their molar ratio is 1:2-4. The total concentration is 0.001-0.01 mol / L. Itaconic acid, acrylic acid or its derivatives in the technical solution improve the stereoregularity and oxidation reaction rate of PAN polymer, the type and concentration of redox initiator will affect the molecular weight, molecular weight distribution, chain end, etc. of PAN polymer, azobisisobutyronitrile obtains higher molecular weight and narrower molecular weight distribution, CuBr2 and TPMA form a coordination complex [Cu(TPMA)]Br2 in water, the complex undergoes coordination reaction with free radicals of acrylonitrile and comonomer, controls the number and activity of free radicals, thereby controls the rate and conversion rate of polymerization reaction, and at the same time the complex undergoes coordination reaction with molecules of acrylonitrile and comonomer, controls the chain segments and chain length of the polymer, thereby controls the molecular weight and molecular weight distribution of the polymer, the molar ratio and total concentration of CuBr2 and TPMA are set, thus ensuring the stability and reactivity of the complex, while avoiding the influence of excessive copper salt and ligand on the purity and solubility of the polymer.
[0019] In a preferred implementation, the polymerization reaction temperature is 30-80° C., the polymerization pressure is 0.1-0.5 MPa, and the polymerization time is 1-10 h.
[0020] In a preferred implementation, the solvent in step S2 is dimethyl sulfoxide, the dissolution temperature is 60-120°C, the dissolution time is 0.5-5h, and the prepared spinning solution has the following indicators: solid content is 18.5-21%, intrinsic viscosity is 1.75-1.9dl / g, and pH value is 8.5-10. The dimethyl sulfoxide solvent used in this technical solution has high solubility, low boiling point, good dissolution mechanism and good solution performance, and is suitable for preparing high molecular weight PAN spinning solution. The prepared spinning solution is transparent, free of impurities and bubbles.
[0021] In a preferred implementation, the metering pump in step S3 adopts a high-precision gear pump with a pump volume of 15-30cc, the filter adopts a metal disc type with a filtration accuracy of 1-3μm, the number of spinneret holes of the spinneret is 1000-4000, the pore size is 0.05-0.2mm, the spinning speed is 5-20m / min, the spinning temperature is 20-40°C, the air layer height is 2-6mm, and the air layer temperature is 18-22°C.
[0022] This technical solution accurately measures the volume of the spinning solution to ensure the fineness index of the original silk, and uses a filter to filter impurities in the system. The spinning solution is converted into a thin stream of raw liquid after passing through the spinneret of the spinneret. The thin stream sprayed by the spinneret is uniform, without interruption and dripping, ensuring stable production operation. The air layer used ensures the stability of the spraying of the raw liquid thin stream; the raw liquid thin stream in the air layer section is highly stretched by 2-4 times.
[0023] In a preferred implementation, the microfluidic chip in step S3 is a multilayer structure, and each layer of the chip is provided with a plurality of spinnerets, and the aperture, number of holes and arrangement of each spinneret can be adjusted as needed to achieve control of the gradient nanostructure of the fiber; the working principle of the microfluidic chip is expressed by the following function formula:
[0024] The flow rate and flow rate of the fluid are related to the hole diameter, number of holes and arrangement of the spinneret, and are calculated using the following formula:
[0025]
[0026] Among them, Q is the total flow, q i is the flow rate of the i-th spinneret, n is the number of spinnerets, d i is the aperture of the ith spinneret, ΔP is the pressure difference, μ is the viscosity of the fluid, and L is the length of the spinneret;
[0027] The streamlines and flow patterns of the fluid are related to the arrangement and relative positions of the spinnerets and can be described by the following function:
[0028]
[0029] Where v is the velocity vector of the fluid, x, y, z are the spatial coordinates, and r i and r j is the position vector of the i-th and j-th spinnerets, θ ij is the angle between the ith and jth spinnerets.
[0030] The gradient nanostructure of the fiber is related to the flow velocity, flow rate, streamline and flow pattern of the fluid, which can be expressed by the following function:
[0031] D(x,y,z)=g(Q,v,f),
[0032] Where D is the diameter of the fiber, x, y, z are spatial coordinates, Q is the total flow rate, v is the velocity vector of the fluid, and f is a function of the fluid's streamlines and flow patterns.
[0033] In a preferred embodiment, the coagulation bath is a mixed liquid of dimethyl sulfoxide and deionized water, the dimethyl sulfoxide concentration is 25-40%, and the coagulation bath temperature is 2-7°C; in the coagulation bath, the original liquid stream is transformed into primary fibers through bidirectional diffusion. Under this process condition, the bidirectional diffusion is stable and uniform, and the primary fibers are relatively dense.
[0034] Under the preferred implementation, the water washing in step S4 adopts multi-stage water washing with deionized water, and the water washing temperature is distributed in a gradient of 30-55°C; the water bath temperature of the hot water drawing is 60-80°C, the fiber is stretched 2-4 times by a high factor, the oiling agent adopts amino-modified silicone oil, the oil concentration is 3-5%, and the temperature is 20-25°C; after water washing, the residual rate of dimethyl sulfoxide in the fiber is low, wherein the hot water drawing is carried out in two hot water tanks, with one drawing before and after, and the fiber stretching multiple is high, which fully improves the mechanical properties of the fiber, and no lint is produced after the fiber is stretched by a high factor.
[0035] In a preferred implementation, the drying uses 1.6MPa medium-pressure steam, sets different steam pressures, multi-stage heating of the steam hot roller, a roller temperature gradient distribution of 140-180°C, and a drying temperature gradient distribution, so as to quickly remove moisture at a high spinning speed and densify the fiber structure.
[0036] In a preferred implementation, the steam stretching uses 1.6MPa medium-pressure steam, and the secondary decompression is 0.4-0.7MPa steam; the fiber is stretched 3-5 times at a high ratio in a steam environment, and the winding is to wind the fiber into a spindle-shaped raw yarn through a winding machine; this technical solution fully removes moisture from the steam, stretches the fiber at a high ratio in the steam, and fully improves the crystallinity and orientation of the fiber.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] (1) After the process of each step of the method of the present invention is matched, the production operation is stable, and stable and continuous production can be achieved. The ultra-high performance precursor produced has a dense internal structure, no defects, no hairy silk in appearance, a smooth surface, good bundling, and no single fiber adhesion; the physical and chemical performance indicators of the produced precursor are: fineness 0.67-0.75dtex, breaking strength>9CN / dtex, modulus>150CN / dtex, oil content 0.8-1.3%, and dimethyl sulfoxide residual rate <300PPM; wherein the breaking strength and modulus indicators are high; the ultra-high performance precursor produced by the preparation method is carbonized to produce ultra-high performance carbon fiber, and the physical and chemical indicators of the carbon fiber are strength>6300MPa and modulus greater than 290GPa; the T1000 qualified rate can be>90%, and the T1100 qualified rate can be>60%;
[0039] (2) The present invention uses the ATRP reaction to achieve precise control of parameters such as the molecular structure, molecular weight, molecular weight distribution, comonomer content, and stereoregularity of the PAN polymer, thereby improving the carbon content, cyclization rate, thermal stability, and other properties of the PAN polymer, and providing high-quality precursor materials for the preparation of ultra-high performance carbon fibers;
[0040] (3) The present invention adopts a microfluidic chip for spinning, which can achieve precise control of the PAN spinning solution, thereby obtaining fibers with different diameters, different flow rates, different flow patterns and different streamlines, avoiding the micropore defects and skin-core structure generated in the traditional spinning process, and improving the mechanical properties, thermal stability and surface properties of the original fiber; by adopting a multi-layer microfluidic chip, the gradient nanostructure of the fiber can be controlled, thereby affecting the molecular orientation, molecular chain spacing, crystal structure and defect structure of the fiber, and further affecting the mechanical properties, thermal stability and surface properties of the fiber, and preparing ultra-high performance carbon fiber. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0042] In order to enable those skilled in the art to better understand the technical solution, the present invention is described in detail below in conjunction with embodiments. The description in this section is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention.
[0043] like Figure 1 As shown in the process flow chart, the raw materials of the present invention are subjected to various treatments to obtain ultra-high performance carbon fiber precursor, and the specific treatment process is described in the following embodiments.
[0044] Embodiment 1:
[0045] A method for preparing ultra-high performance carbon fiber precursor, comprising the following steps:
[0046] S1. Polymerization: In water containing acrylonitrile (AN) and itaconic acid (IA), azobisisobutyronitrile (AIBN) as a redox initiator, and CuBr2 and TPMA as copper salt and ligand were added in a molar ratio of 1:3 and a total concentration of 0.005 mol / L to form a heterogeneous reaction system for polymerization. The polymerization temperature was 50°C, the polymerization pressure was 0.2 MPa, and the polymerization time was 5 h. After the reaction was completed, PAN polymer powder was obtained by filtering, washing and drying. The mass fraction of itaconic acid was 7%, and the mass ratio of acrylonitrile to itaconic acid was 13:1. The chemical reaction equation involved is as follows:
[0047]
[0048] S2. Preparation of spinning solution: dissolving the obtained PAN polymer powder in dimethyl sulfoxide (DMSO) solvent at a dissolution temperature of 80° C. for 2 h to prepare a spinning solution. The spinning solution has the following indicators: solid content of 20%, intrinsic viscosity of 1.8 dl / g, and pH value of 9;
[0049] S3, spinning: the spinning solution is sent into the microfluidic chip through a precision metering pump, and then reaches the spinneret after passing through the filter, and a thin stream of the stock solution is ejected, and after passing through a section of air layer, it enters the coagulation bath, and forms nascent fibers in the coagulation bath. The metering pump adopts a high-precision gear pump with a pump volume of 20cc, and the filter adopts a metal disc type with a filtration accuracy of 2μm. The spinneret has 1000 holes, a pore size of 0.1mm, a spinning speed of 5m / min, and a spinning temperature of 40°C. The air layer height is 4mm, and the air layer temperature is 20°C. The microfluidic chip is a multi-layer structure, and each layer of the chip is provided with 10 spinnerets. The pore size, number of holes and arrangement of each spinneret can be adjusted as needed to achieve the control of the gradient nanostructure of the fiber. The coagulation bath is a mixed liquid of dimethyl sulfoxide and deionized water, the dimethyl sulfoxide concentration is 30%, and the coagulation bath temperature is 5°C;
[0050] S4, drawing preparation: the obtained spun fiber is subjected to water washing, hot water drawing, oiling, drying, steam drawing and winding to obtain ultra-high performance carbon fiber precursor, wherein the water washing adopts multi-stage water washing with deionized water, and the washing temperature is gradually increased from 30°C to 55°C in a gradient distribution; the water bath temperature of the hot water drawing is 60°C, the fiber is stretched 3 times, the oiling agent adopts amino-modified silicone oil, the oil concentration is 4%, the temperature is 22°C, the drying adopts 1.6MPa medium-pressure steam, different steam pressures are set, the steam hot roller is heated in multiple stages, the roller temperature is gradually increased from 140°C to 180°C in a gradient distribution, the steam drawing adopts 1.6MPa medium-pressure steam, and the secondary decompression is 0.6MPa steam; the fiber is stretched 4 times in a steam environment, and the winding is to roll the fiber into ingot-shaped precursor by a winder.
[0051] Embodiment 2:
[0052] A method for preparing ultra-high performance carbon fiber precursor, comprising the following steps:
[0053] S1. Polymerization: In water containing acrylonitrile (AN) and acrylic acid (AA), azobisisobutyronitrile (AIBN) as a redox initiator, and CuBr2 and TPMA as copper salt and ligand are added in a molar ratio of 1:2 and a total concentration of 0.01 mol / L to form a heterogeneous reaction system for polymerization. The polymerization temperature is 80°C, the polymerization pressure is 0.5 MPa, and the polymerization time is 2 h. After the reaction is completed, PAN polymer powder is obtained by filtering, washing and drying. The mass fraction of acrylic acid is 2%, and the mass ratio of acrylonitrile to acrylic acid is 40:1. The chemical reaction equation involved is as follows:
[0054]
[0055] S2. Preparation of spinning solution: dissolving the obtained PAN polymer powder in dimethyl sulfoxide (DMSO) solvent at a dissolution temperature of 120° C. for 0.5 h to prepare a spinning solution. The spinning solution has the following indicators: solid content of 18.5%, intrinsic viscosity of 1.75 dl / g, and pH value of 8.5;
[0056] S3, spinning: the spinning solution is sent into the microfluidic chip through a precision metering pump, and then reaches the spinneret after passing through the filter, and a thin stream of the stock solution is ejected, and after passing through a section of air layer, it enters the coagulation bath, and forms primary fibers in the coagulation bath. The metering pump adopts a high-precision gear pump with a pump volume of 30cc, and the filter adopts a metal disc type with a filtration accuracy of 3μm. The spinneret has 3000 holes, a pore size of 0.2mm, a spinning speed of 15m / min, and a spinning temperature of 30°C. The air layer height is 6mm, and the air layer temperature is 18°C. The microfluidic chip is a multi-layer structure, and each layer of the chip is provided with 8 spinnerets. The pore size, number of holes and arrangement of each spinneret can be adjusted as needed to achieve the control of the gradient nanostructure of the fiber. The coagulation bath is a mixed liquid of dimethyl sulfoxide and deionized water, the dimethyl sulfoxide concentration is 25%, and the coagulation bath temperature is 7°C;
[0057] S4, drawing preparation: the obtained spun fiber is subjected to water washing, hot water drawing, oiling, drying, steam drawing and winding to obtain ultra-high performance carbon fiber precursor, wherein the water washing adopts multi-stage water washing with deionized water, and the washing temperature is gradually increased from 30°C to 55°C in a gradient distribution; the water bath temperature of the hot water drawing is 80°C, the fiber is stretched 4 times, the oiling agent adopts amino-modified silicone oil, the oil concentration is 3%, the temperature is 25°C, the drying adopts 1.6MPa medium-pressure steam, different steam pressures are set, the steam hot roller is heated in multiple stages, the roller temperature is gradually increased from 140°C to 180°C in a gradient distribution, the steam drawing adopts 1.6MPa medium-pressure steam, and the secondary decompression is 0.4MPa steam; the fiber is stretched 3 times in a steam environment, and the winding is to roll the fiber into ingot-shaped precursor by a winder.
[0058] Embodiment 3:
[0059] A method for preparing ultra-high performance carbon fiber precursor, comprising the following steps:
[0060] S1. Polymerization: In water containing acrylonitrile (AN) and itaconic acid (IA), azobisisobutyronitrile (AIBN) as a redox initiator, and CuBr2 and TPMA as copper salt and ligand are added in a molar ratio of 1:4 and a total concentration of 0.001 mol / L to form a heterogeneous reaction system for polymerization. The polymerization temperature is 30°C, the polymerization pressure is 0.1 MPa, and the polymerization time is 8 h. After the reaction is completed, PAN polymer powder is obtained by filtering, washing and drying; the mass fraction of itaconic acid is 5%, and the mass ratio of acrylonitrile to itaconic acid is 20:1. The chemical reaction equation involved is as follows:
[0061]
[0062] S2. Preparation of spinning solution: dissolving the obtained PAN polymer powder in dimethyl sulfoxide (DMSO) solvent at a dissolution temperature of 60° C. for 5 h to prepare a spinning solution. The spinning solution has the following indicators: solid content of 21%, intrinsic viscosity of 1.9 dl / g, and pH value of 10;
[0063] S3, spinning: the spinning solution is sent into the microfluidic chip through a precision metering pump, and then reaches the spinneret after passing through the filter, and a thin stream of the stock solution is ejected, and after passing through a section of air layer, it enters the coagulation bath, and forms primary fibers in the coagulation bath. The metering pump adopts a high-precision gear pump with a pump volume of 15cc, and the filter adopts a metal disc type with a filtration accuracy of 1μm. The number of holes of the spinneret spinneret is 4000, the pore size is 0.05mm, the spinning speed is 20m / min, the spinning temperature is 20℃, the air layer height is 2mm, and the air layer temperature is 22℃. The microfluidic chip is a multi-layer structure, and each layer of the chip is provided with 10 spinnerets. The pore size, number of holes and arrangement of each spinneret can be adjusted as needed to achieve the control of the gradient nanostructure of the fiber. The coagulation bath is a mixed liquid of dimethyl sulfoxide and deionized water, the dimethyl sulfoxide concentration is 40%, and the coagulation bath temperature is 2℃;
[0064] S4, drawing preparation: the obtained spun fiber is subjected to water washing, hot water drawing, oiling, drying, steam drawing and winding to obtain ultra-high performance carbon fiber precursor, wherein the water washing adopts multi-stage water washing with deionized water, and the washing temperature is gradually increased from 30°C to 55°C in a gradient distribution; the water bath temperature of the hot water drawing is 65°C, the fiber is stretched 2 times, the oiling agent adopts amino-modified silicone oil, the oil concentration is 5%, the temperature is 20°C, the drying adopts 1.6MPa medium-pressure steam, different steam pressures are set, the steam hot roller is heated in multiple stages, the roller temperature is gradually increased from 140°C to 180°C in a gradient distribution, the steam drawing adopts 1.6MPa medium-pressure steam, and the secondary decompression is 0.7MPa steam; the fiber is stretched 5 times in a steam environment, and the winding is to roll the fiber into ingot-shaped precursor by a winder.
[0065] Embodiment 4:
[0066] First, the relationship between the flow rate and flow rate of the fluid and the hole diameter, number of holes and arrangement of the spinneret. This relationship is calculated using the following formula:
[0067]
[0068] Where Q is the total flow rate, qi is the flow rate of the ith spinneret, n is the number of spinnerets, di is the aperture of the ith spinneret, ΔP is the pressure difference, μ is the viscosity of the fluid, and L is the length of the spinneret.
[0069] This formula is derived from the Hagen-Poiseuille flow equation. The Hagen-Poiseuille flow equation describes the laminar flow of a Newtonian fluid in a circular pipe under a constant pressure difference. It can be written as:
[0070]
[0071] Where q is the flow rate, d is the pipe diameter, ΔP is the pressure difference across the pipe, μ is the viscosity of the fluid, and L is the length of the pipe.
[0072] Since there are multiple spinnerets on the microfluidic chip, each spinneret can be regarded as a circular pipe, so the flow rate of each spinneret is calculated using the above formula, and then they are added together to get the total flow rate. This is the derivation process of the above formula.
[0073] Next, the relationship between the fluid streamlines and flow patterns and the arrangement and relative positions of the spinnerets is described by the following function:
[0074]
[0075] Where v is the velocity vector of the fluid, x, y, z are the spatial coordinates, and r i and r j is the position vector of the i-th and j-th spinnerets, θ ij is the angle between the ith and jth spinnerets.
[0076] This function is derived based on the superposition principle in fluid mechanics. The superposition principle means that in a complex flow field, if the flow is decomposed into several simple flows, the velocity vectors of each simple flow are added together to obtain the velocity vector of the complex flow. For example, if there are two spinnerets, their position vectors are r1 and r2, and their velocity vectors are v1 and v2, then the velocity vector v at any point is written as:
[0077] v=v1+v2
[0078] Among them, v1 and v2 can be calculated using the following formula:
[0079]
[0080]
[0081] Among them, r is the position vector of any point, q1 and q2 are the flow rates of the two spinnerets, and d1 and d2 are the apertures of the two spinnerets.
[0082] Since there are multiple spinnerets on the microfluidic chip, each spinneret can be regarded as a point source, so the flow velocity vector of each spinneret is calculated using the above formula, and then they are added together to obtain the flow velocity vector at any point. This is the derivation process of the above function.
[0083] Finally, the relationship between the gradient nanostructure of the fiber and the flow velocity, flow rate, streamline and flow pattern of the fluid is expressed by the following function:
[0084] D(x,y,z)=g(Q,v,f)
[0085] Where D is the diameter of the fiber, x, y, z are spatial coordinates, Q is the total flow rate, v is the velocity vector of the fluid, and f is a function of the fluid's streamlines and flow patterns.
[0086] This function is derived based on the stretching mechanism of nanofibers. The stretching mechanism of nanofibers means that after the fluid is ejected from the spinneret, due to the air resistance and surface tension, the fluid will be stretched in the air layer, thereby reducing the diameter of the fiber. This process is described by the following formula:
[0087]
[0088] Where D is the diameter of the fiber, D0 is the hole diameter of the spinneret, and λ is the draw ratio, which is calculated using the following formula:
[0089]
[0090] Among them, v is the velocity of the fluid in the air layer, and v0 is the velocity of the fluid ejected from the spinneret.
[0091] Since there are multiple spinnerets on the microfluidic chip, the aperture, flow rate and arrangement of each spinneret can be adjusted, so the gradient nanostructure of the fiber can be controlled by controlling the speed of the fluid in the air layer.
[0092] Comparative Example 1:
[0093] The difference between this comparative example and Example 1 is that the polymerization reaction adopts a traditional free radical polymerization method, without adding copper salt and ligand, and only adding azobisisobutyronitrile as an initiator, and its amount is 1% (relative to the total mass of AN and IA).
[0094] Comparative Example 2:
[0095] The difference between this comparative example and Example 1 is that the spinning method adopts the traditional wet spinning method, does not use a microfluidic chip, but uses an ordinary spinneret.
[0096] The physical and chemical properties of the ultra-high performance carbon fiber precursors prepared in the above Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in the following table:
[0097] Table 1
[0098]
[0099] The ultra-high performance precursors produced by the preparation methods of Examples 1-3 and Comparative Examples 1-2 are carbonized to produce ultra-high performance carbon fibers. The test results of the physical and chemical indicators of the carbon fibers are shown in the following table.
[0100] Table 2
[0101]
[0102] It should be noted that, in this article, the terms include, contain or any other variant thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. Specific examples are used in this article to illustrate the principle and implementation of the technical solution of the present invention. The above examples are only used to help understand the method of the present invention and its core idea. The above are only preferred implementations of the present invention. It should be pointed out that due to the limitations of textual expression and the objective existence of infinite specific structures, for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements, modifications or changes can be made, and the above technical features can also be combined in an appropriate manner; these improvements, modifications, changes or combinations, or the direct application of the concept and technical solution of the invention to other occasions without improvement, should be regarded as the protection scope of the present invention.
Claims
1. A method for preparing ultra-high performance carbon fiber precursor, characterized in that: The following steps are involved: S1. Polymerization: Add a redox initiator, copper salt and ligand TPMA to water containing acrylonitrile and comonomer to form a heterogeneous reaction system for polymerization. After the reaction is completed, filter, wash and dry to obtain PAN polymer powder. The comonomer is itaconic acid, acrylic acid or its derivatives, and its content is 2-7% of the mass of PAN polymer. The mass ratio of acrylonitrile to the comonomer is 9-50:
1. The redox initiator is azobisisobutyronitrile. The copper salt and ligand are CuBr2 and TPMA, and their molar ratio is 1:2-4. The total concentration is 0.001-0.01 mol / L. The chemical reaction equation involved is as follows: ; S2, spinning solution preparation: dissolving the obtained PAN polymer powder in a solvent to prepare a spinning solution; S3, spinning: the spinning solution is sent into the microfluidic chip through a precision metering pump, and then reaches the spinneret after passing through a filter, and a thin stream of the stock solution is ejected, and enters the coagulation bath after passing through a section of air layer, and the primary fiber is formed in the coagulation bath. The microfluidic chip is a multi-layer structure, and each layer of the chip is provided with a plurality of spinnerets. The aperture, number of holes and arrangement of each spinneret are adjusted as needed to realize the control of the gradient nanostructure of the fiber; the working principle of the microfluidic chip is expressed by the following function formula: The flow rate and flow rate of the fluid are related to the hole diameter, number of holes and arrangement of the spinneret, and are calculated using the following formula: , Among them, Q is the total flow, q i is the flow rate of the i-th spinneret, n is the number of spinnerets, d i is the aperture of the ith spinneret, ΔP is the pressure difference, μ is the viscosity of the fluid, and L is the length of the spinneret; The streamlines and flow patterns of the fluid are related to the arrangement and relative positions of the spinnerets and can be described by the following function: , Where v is the velocity vector of the fluid, x, y, z are the spatial coordinates, and r i and r j is the position vector of the i-th and j-th spinnerets, θ ij is the angle between the ith and jth spinnerets; The gradient nanostructure of the fiber is related to the flow velocity, flow rate, streamline and flow pattern of the fluid, which can be expressed by the following function: , Where D is the diameter of the fiber, x, y, z are spatial coordinates, Q is the total flow rate, v is the velocity vector of the fluid, and f is a function of the fluid streamline and flow pattern; S4, drawing preparation: The obtained spun fiber is subjected to water washing, hot water drawing, oiling, drying, steam drawing and winding to obtain ultra-high performance carbon fiber precursor.
2. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: The polymerization reaction temperature is 30-80° C., the polymerization pressure is 0.1-0.5 MPa, and the polymerization time is 1-10 h.
3. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: The solvent in step S2 is dimethyl sulfoxide, the dissolution temperature is 60-120° C., the dissolution time is 0.5-5 h, and the prepared spinning solution has the following indicators: solid content is 18.5-21%, intrinsic viscosity is 1.75-1.9 dl / g, and pH value is 8.5-10.
4. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: In the step S3, the metering pump adopts a high-precision gear pump with a pump volume of 15-30cc, the filter adopts a metal disc type with a filtration accuracy of 1-3μm, the number of spinneret holes of the spinneret is 1000-4000, the pore size is 0.05-0.2mm, the spinning speed is 5-20m / min, the spinning temperature is 20-40°C, the air layer height is 2-6mm, and the air layer temperature is 18-22°C.
5. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: The coagulation bath is a mixed liquid of dimethyl sulfoxide and deionized water, the concentration of dimethyl sulfoxide is 25-40%, and the coagulation bath temperature is 2-7°C.
6. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: In step S4, the water washing adopts multi-stage water washing with deionized water, and the water washing temperature is distributed in a gradient of 30-55°C; the hot water drawing water bath temperature is 60-80°C, the fiber is stretched 2-4 times, and the oiling agent adopts amino-modified silicone oil, the oil concentration is 3-5%, and the temperature is 20-25°C.
7. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: The drying adopts 1.6MPa medium-pressure steam, sets different steam pressures, and uses a steam hot roller for multi-stage heating, with a roller temperature gradient distribution of 140-180°C.
8. The method for preparing ultra-high performance carbon fiber precursor according to claim 1, characterized in that: The steam drawing uses 1.6MPa medium-pressure steam, and the secondary decompression is 0.4-0.7MPa steam; the fiber is stretched 3-5 times under the steam environment, and the winding is to wind the fiber into a spindle-shaped raw silk through a winding machine.