A kind of amino silicone oil softener and its preparation method and application

By preparing a quaternized modified amino silicone oil softener, the yellowing problem of amino silicone oil under the action of light, heat and oxygen is solved, and its hydrophilicity and stability are improved, thereby protecting the softness and whiteness of fabrics. Suitable for finishing of cellulose fibers and their blended fabrics.

CN118007437BActive Publication Date: 2024-10-11GUANGDONG RUNXIANG FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410098838.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-10-11
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

Existing amino silicone softeners are prone to oxidation and yellowing when exposed to light, heat, and oxygen, which affects the appearance of fabrics. They also lack hydrophilicity and air permeability, making it difficult to impart softness and whiteness protection to fabrics at the same time.

Method used

By mixing and heating α,ω-dihydroxypolydimethylsiloxane, amino coupling agent and end-capping agent, adding an alkaline catalyst for reaction, and then mixing with quaternizing reagent and emulsifier to adjust the pH value, quaternary ammonium siloxane is prepared. Ammonium-modified amino silicone oil softener reduces amino active hydrogen, introduces hydrophilic groups, reduces interfacial tension, and improves emulsification effect.

Benefits of technology

The prepared amino silicone oil softener has low yellowing, excellent hydrophilicity and stability, can impart softness and whiteness in fabric finishing, and is easy for industrial production and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004679487880000091
    Figure BDA0004679487880000091
  • Figure BDA0004679487880000101
    Figure BDA0004679487880000101
  • Figure BDA0004679487880000102
    Figure BDA0004679487880000102
Patent Text Reader

Abstract

The invention relates to an amino silicone oil softener and a preparation method and application thereof, belonging to the technical field of fabric treatment. The quaternary ammonium modified amino silicone oil fabric softener prepared by the method provided by the invention can be used for soft finishing of cellulose fibers and blended fabrics thereof, and imparts excellent hydrophilic effect to the textiles, while reducing the influence on yellowing of the textiles; the prepared quaternary ammonium modified amino silicone oil fabric softener has stable properties and is easy to produce, store and use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric treatment, and in particular relates to an amino silicone oil softener and a preparation method and application thereof. Background Art

[0002] With the development of economy and the improvement of people's living standards, the public's functional requirements for textiles are also increasing. Specifically, in addition to meeting the basic functions such as warmth and beauty, people also pursue special functions such as comfort, softness, antibacterial properties, antistatic properties, waterproof and oil-proof properties, and wrinkle resistance of textiles.

[0003] Finishing is generally the last chemical processing step of fabrics. Finishing auxiliaries are applied to fabrics with water or other solvents as the medium, and then dried and baked to keep the effective ingredients in the auxiliaries on the fabrics to play their role. Softening finishing is an important finishing step in the textile printing and dyeing process. After desizing, bleaching, washing and other processes, the fabric will become rough. Microemulsions are prepared using organopolysiloxane to form organosilicon softeners, and the fabrics are finished so that the polysiloxane can form a film on the fiber surface and cover the rough areas on the fiber surface, which reduces the friction coefficient of the fiber surface and makes the fabric feel soft and smooth.

[0004] The commonly used type of silicone softener is to introduce other reactive groups such as amino, carboxyl, epoxy, polyether and other groups into the silicone molecular chain, thereby giving silicone oil new properties, such as amino silicone oil, epoxy silicone oil, carboxyl silicone oil, etc. Among them, amino silicone oil is the most widely used silicone oil in the market. Its amino group has strong polarity and can firmly bond with fibers, giving fabrics excellent soft feel. However, due to the presence of amino groups, especially primary amino groups, in amino silicone oil, it is very easy to oxidize and produce yellowing when exposed to light, heat, oxygen and other conditions, affecting the appearance of the fabric or changing the color of colored fabrics. In addition, there is a lack of hydrophilic groups in the structure of amino silicone oil. Generally speaking, in addition to the superior feel, fabrics finished with amino silicone oil have poor other properties such as hydrophilicity and air permeability.

[0005] Therefore, it is of great significance to provide a softener that can simultaneously impart softness and hydrophilicity to fabrics and has little effect on fabric whiteness. Summary of the invention

[0006] The purpose of the present invention is to overcome the problems existing in the above-mentioned prior art and to provide an amino silicone oil softener and a preparation method and application thereof.

[0007] The present invention is achieved through the following technical solutions:

[0008] The present invention provides a method for preparing an amino silicone oil softener, comprising the following steps:

[0009] (1) Mixing α,ω-dihydroxy polydimethylsiloxane, amino coupling agent aminoethylaminopropylmethyldimethoxysilane and end-capping agent, heating to 75°C-80°C, adding alkaline catalyst, continuing to heat to 100°C-110°C, and keeping the temperature for 3h-4h to obtain aminosilicone oil intermediate;

[0010] (2) mixing the aminosilicone oil intermediate obtained in step (1) with a quaternary ammonium agent and an organic solvent, heating to 80° C.-90° C., reacting for 2 h-4 h, to obtain a quaternary ammonium modified aminosilicone oil;

[0011] (3) mixing the quaternary ammonium modified amino silicone oil obtained in step (2) and the emulsifier, stirring evenly, adjusting the pH value to 4-6, and filtering to obtain the amino silicone softener;

[0012] In the step (3), the emulsifier comprises the following components in percentage by mass: 40%-60% of isotridecyl alcohol polyoxyethylene ether, 20%-40% of isotridecyl alcohol polyoxyethylene ether, 10%-20% of fatty alcohol polyoxyethylene ether, 5%-10% of fatty alcohol polyoxyethylene ether carboxylic acid, and 1%-5% of diethylene glycol monobutyl ether.

[0013] The quaternary ammonium modified amino silicone oil softener of the present invention has a certain low yellowing property due to the reduction of active hydrogen on the amino group, and has little effect on the whiteness of the fabric; at the same time, the hydrophilic group hydroxyl group is introduced, which can give the fabric excellent hydrophilicity; and by using a composite emulsifier with a specific ratio, the interfacial tension is reduced, so that the interaction between oil and water molecules is reduced, thereby achieving mutual mixing of oil and water, increasing the emulsification effect, and improving the easy emulsification, so that the obtained amino silicone oil softener has excellent stability and can synergistically improve the softness, hydrophilicity and whiteness of the treated fabric. The preparation method of the present invention is simple, cost-saving, easy to industrially produce, and the product is easy to use.

[0014] Preferably, in step (1), the mass ratio of the α,ω-dihydroxypolydimethylsiloxane to the amino coupling agent and the end-capping agent is (80-98): (1-5): (0.5-3).

[0015] Preferably, in step (1), the capping agent includes at least one of hexamethyldisiloxane and octamethyltrisiloxane.

[0016] Preferably, in step (1), the alkaline catalyst comprises at least one of potassium hydroxide and tetramethylammonium hydroxide.

[0017] Preferably, in step (1), the amount of the alkaline catalyst added is 0.03%-0.1% of the mass of α,ω-dihydroxypolydimethylsiloxane.

[0018] More preferably, the alkaline catalyst is a potassium hydroxide aqueous solution with a mass concentration of 20%-50% and / or a tetramethylammonium hydroxide aqueous solution with a mass concentration of 20%-50%.

[0019] Preferably, in step (2), the quaternizing agent includes 2,3-epoxypropyltrimethylammonium chloride.

[0020] Preferably, in step (2), the organic solvent comprises isopropanol.

[0021] Preferably, in step (2), the mass ratio of the aminosilicone oil intermediate to the quaternary ammonium agent and the organic solvent is (60-80):(4-6):(20-30).

[0022] More preferably, the mass ratio of the aminosilicone oil intermediate to the quaternary ammonium agent and the organic solvent is 70:5:25.

[0023] Preferably, in the step (3), the mass ratio of the quaternary ammonium modified amino silicone oil to the emulsifier is (1-4):1.

[0024] More preferably, the mass ratio of the quaternary ammonium modified amino silicone oil to the emulsifier is 2:1.

[0025] Preferably, in step (3), the pH value is adjusted to 4-6 by adding acetic acid and water.

[0026] Another object of the present invention is to provide an amino silicone oil softener prepared by the preparation method of the amino silicone oil softener.

[0027] Another object of the present invention is to provide application of the amino silicone oil softener in fabric finishing.

[0028] The present invention has the following beneficial effects: the quaternary ammonium modified amino silicone oil softener prepared by the amino silicone oil softener preparation method of the present invention can be used for soft-style finishing of cellulose fibers and blended fabrics thereof, etc., can give the fabric excellent softness and hydrophilicity during the finishing of the fabric, has little effect on the whiteness of the fabric, has excellent stability, is easy to produce, store and use, and is conducive to industrial production and application. DETAILED DESCRIPTION

[0029] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0030] Unless otherwise specified, the experimental methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels.

[0031] The α,ω-dihydroxy polydimethylsiloxane in the following examples and comparative examples is PMX-0156, purchased from Dow Corning Silicones Co., Ltd., and has a viscosity of 50-120 mPa·s at 25°C;

[0032] The brand of aminoethylaminopropylmethyldimethoxysilane is KH-602, which was purchased from Guangzhou Yuanda New Materials Co., Ltd.

[0033] The brand of hexamethyldisiloxane is MM, which was purchased from Shenzhen Jiefengchuan Chemical Technology Co., Ltd.;

[0034] The brand number of 2,3-epoxypropyltrimethylammonium chloride is 3033-77-0, which was purchased from Guangzhou Yuanda New Materials Co., Ltd.;

[0035] The brand of isomeric tridecanol polyoxyethylene ether is TO-9, which was purchased from BASF China Co., Ltd.

[0036] The brand of isomeric decanol polyoxyethylene ether is XP-50, which was purchased from BASF China Co., Ltd.;

[0037] The brand of fatty alcohol polyoxyethylene ether is AEO-9, which was purchased from BASF China Co., Ltd.;

[0038] The brand of fatty alcohol polyoxyethylene ether carboxylic acid is AEC-9H, which was purchased from Zhonghe Chemical (Shandong) Co., Ltd.;

[0039] The brand number of diethylene glycol monobutyl ether is 112-34-5, which was purchased from Guangzhou Chemical Reagent Factory;

[0040] The brand of alkyl glycoside is APG-25, which was purchased from Guangzhou Jinglong Technology Co., Ltd.;

[0041] Allyltrimethylammonium chloride was purchased from Shanghai Lianji Chemical Co., Ltd. with the brand number of 1516-27-4;

[0042] The brand of aminoethylaminopropyltrimethoxysilane is KH-792, which was purchased from Hangzhou Jessica Chemical Co., Ltd.;

[0043] The commercially available amino silicone oil of Comparative Example 1 is of brand H8001, purchased from Guangzhou Honghua Chemical Co., Ltd.

[0044] Example 1

[0045] A method for preparing an amino silicone oil softener comprises the following steps:

[0046] (1) Add 485 g of α,ω-dihydroxypolydimethylsiloxane, 11.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0047] (2) Add 340 g of the aminosilicone oil intermediate obtained in step (1), 21.5 g of 2,3-epoxypropyltrimethylammonium chloride, and 138.5 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0048] (3) 100 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 344.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0049] In the step (3), the emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0050] Example 2

[0051] A method for preparing an amino silicone oil softener comprises the following steps:

[0052] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0053] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of 2,3-epoxypropyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0054] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0055] In the step (3), the emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0056] Example 3

[0057] A method for preparing an amino silicone oil softener comprises the following steps:

[0058] (1) Add 470 g of α,ω-dihydroxypolydimethylsiloxane, 26.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0059] (2) Add 375 g of the aminosilicone oil intermediate obtained in step (1), 27.5 g of 2,3-epoxypropyltrimethylammonium chloride, and 97.5 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0060] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 45 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 344.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0061] In the step (3), the emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0062] Example 4

[0063] A method for preparing an amino silicone oil softener comprises the following steps:

[0064] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0065] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of 2,3-epoxypropyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0066] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0067] In the step (3), the emulsifier comprises the following components in percentage by mass: 60% of isomeric tridecanol polyoxyethylene ether, 20% of isomeric decanol polyoxyethylene ether, 14% of fatty alcohol polyoxyethylene ether, 5% of fatty alcohol polyoxyethylene ether carboxylic acid, and 1% of diethylene glycol monobutyl ether.

[0068] Example 5

[0069] A method for preparing an amino silicone oil softener comprises the following steps:

[0070] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0071] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of 2,3-epoxypropyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0072] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0073] In the step (3), the emulsifier comprises the following components in percentage by mass: 40% of isomeric tridecanol polyoxyethylene ether, 30% of isomeric decanol polyoxyethylene ether, 15% of fatty alcohol polyoxyethylene ether, 10% of fatty alcohol polyoxyethylene ether carboxylic acid, and 5% of diethylene glycol monobutyl ether.

[0074] Comparative Example 1

[0075] A method for preparing an amino silicone oil softener comprises the following steps:

[0076] 110 g of commercially available amino silicone oil and 55 g of emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this comparative example.

[0077] The emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0078] Comparative Example 2

[0079] A method for preparing an amino silicone oil softener comprises the following steps:

[0080] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0081] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of 2,3-epoxypropyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0082] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0083] In the step (3), the emulsifier comprises the following components in percentage by mass: 28% of isomeric tridecanol polyoxyethylene ether, 49% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0084] Comparative Example 3

[0085] A method for preparing an amino silicone oil softener comprises the following steps:

[0086] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0087] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of 2,3-epoxypropyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0088] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0089] In the step (3), the emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of alkyl glycoside, and 3% of diethylene glycol monobutyl ether.

[0090] Comparative Example 4

[0091] A method for preparing an amino silicone oil softener comprises the following steps:

[0092] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropylmethyldimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0093] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of allyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0094] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0095] In the step (3), the emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0096] Comparative Example 5

[0097] A method for preparing an amino silicone oil softener comprises the following steps:

[0098] (1) Add 480 g of α,ω-dihydroxypolydimethylsiloxane, 16.5 g of aminoethylaminopropyltrimethoxysilane, and 3.35 g of hexamethyldisiloxane to a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, mix and stir, heat to 75° C., add 0.75 g of a 20% potassium hydroxide aqueous solution, continue to heat to 110° C., and keep the temperature for 4 hours to obtain an aminosilicone oil intermediate;

[0099] (2) Add 350 g of the aminosilicone oil intermediate obtained in step (1), 25.0 g of 2,3-epoxypropyltrimethylammonium chloride, and 125.0 g of isopropanol into a round-bottom flask equipped with a stirrer, a reflux condenser, and a thermometer, stir and heat to 80° C., and react for 3 h to obtain a quaternary ammonium modified aminosilicone oil;

[0100] (3) 110 g of the quaternary ammonium modified amino silicone oil obtained in step (2) and 55 g of the emulsifier were mixed and vigorously stirred. After stirring evenly, 0.5 g of acetic acid and 334.5 g of water were slowly added and stirred continuously. The pH value was finally controlled to be 4-6 to obtain an amino silicone oil emulsion, which was filtered to obtain the amino silicone oil softener of this embodiment.

[0101] In the step (3), the emulsifier comprises the following components in percentage by mass: 49% of isomeric tridecanol polyoxyethylene ether, 28% of isomeric decanol polyoxyethylene ether, 13% of fatty alcohol polyoxyethylene ether, 7% of fatty alcohol polyoxyethylene ether carboxylic acid, and 3% of diethylene glycol monobutyl ether.

[0102] Performance Testing

[0103] The aminosilicone softener prepared in the above embodiments and comparative examples was used to finish the fabric for performance testing. The experimental method was as follows: pure white knitted cotton cloth was used as the fabric sample, the amount of aminosilicone softener was 50 g / L, the padding method was adopted, and the fabric sample was shaped and dried at 170°C for 90 seconds to obtain the softened fabric sample.

[0104] The fabric samples after softening were subjected to performance tests respectively, and the methods were as follows:

[0105] (1) Softness test: The softness and smoothness are evaluated by hand touch on a scale of 1-5, with 5 being the best and 1 being the worst.

[0106] (2) Hydrophilicity test: It is characterized by static water absorption time. A drop of water is dropped onto the flat surface of the fabric from a height of 2 cm from the fabric using a dropper, and the time taken for the fabric to absorb the water drop is measured.

[0107] (3) Whiteness test: Use a computer colorimeter to measure the whiteness value of the finished sample.

[0108] The test results are shown in Table 1.

[0109] Table 1 Test results of fabric samples after treatment in the embodiments and comparative examples

[0110]

[0111]

[0112] As can be seen from Table 1, the quaternary ammonium modified amino silicone oil softener prepared by the preparation method of the quaternary ammonium modified amino silicone oil softener provided by the present invention can give the fabric excellent softness and hydrophilicity in the fabric finishing, and has little effect on the whiteness of the fabric. Among them, the performance of the quaternary ammonium modified amino silicone oil softener of Example 2 is the most outstanding.

[0113] Stability test

[0114] The amino silicone oil softeners prepared in the above examples and comparative examples were tested for stability. The test conditions were: 80 g / L of amino silicone oil softener, 30 g / L of soda ash, 30 g / L of caustic soda, 10 g / L of sodium sulfate, and 10 g / L of color fixative were added to prepare a solution and observe the phenomenon.

[0115] The stability test results are shown in Table 2.

[0116] Table 2 Stability test results

[0117]

[0118]

[0119] As can be seen from Table 2, the quaternary ammonium modified amino silicone oil softener prepared by the preparation method of the quaternary ammonium modified amino silicone oil softener provided by the present invention has good salt resistance, alkali resistance and color fixing agent stability, indicating that the composite emulsifier of the present invention can greatly improve the stability of the amino silicone oil softener, and the amino silicone oil emulsifier of the present invention is conducive to industrial production and use.

[0120] In addition, it can be seen from Table 1 and Table 2 that the performance of each comparative example is poor. Among them, comparative example 1 uses non-quaternary ammonium modified commercial amino silicone oil, and the obtained softener has poor stability and the softness and hydrophilicity of the treated fabric are significantly reduced; the component content ratio of the emulsifier in comparative example 2 is not good, resulting in a significant reduction in the stability of the softener, and the hydrophilicity of the treated fabric is significantly reduced; in comparative example 3, alkyl glycoside is used to replace fatty alcohol polyoxyethylene ether carboxylic acid, and the synergistic effect with the other components is reduced, resulting in the overall performance of the finished fabric sample is not as good as that of the embodiment; comparative example 4 uses allyl trimethyl ammonium chloride to modify the amino silicone oil, resulting in poor performance of the modified amino silicone oil; comparative example 5 uses aminoethyl aminopropyl trimethoxy silane as the type of amino coupling agent, which cannot make the softener have excellent comprehensive performance.

[0121] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing an amino silicone oil softener, It is characterized in that The following steps are involved: (1) Mixing α,ω-dihydroxy polydimethylsiloxane, amino coupling agent aminoethylaminopropylmethyldimethoxysilane and end-capping agent, heating to 75°C-80°C, adding alkaline catalyst, continuing to heat to 100°C-110°C, and keeping the temperature for 3h-4h to obtain aminosilicone oil intermediate; (2) mixing the aminosilicone oil intermediate obtained in step (1) with a quaternary ammonium agent and an organic solvent, heating to 80° C.-90° C., and reacting for 2 h-4 h to obtain a quaternary ammonium modified aminosilicone oil; the quaternary ammonium agent includes 2,3-epoxypropyltrimethylammonium chloride; (3) mixing the quaternary ammonium modified amino silicone oil obtained in step (2) and the emulsifier, stirring evenly, adjusting the pH value to 4-6, and filtering to obtain the amino silicone softener; In the step (3), the emulsifier comprises the following components in percentage by mass: 40%-60% of isotridecyl alcohol polyoxyethylene ether, 20%-40% of isotridecyl alcohol polyoxyethylene ether, 10%-20% of fatty alcohol polyoxyethylene ether, 5%-10% of fatty alcohol polyoxyethylene ether carboxylic acid, and 1%-5% of diethylene glycol monobutyl ether.

2. The preparation method of amino silicone oil softener according to claim 1, It is characterized in that In the step (1), the mass ratio of the α,ω-dihydroxypolydimethylsiloxane to the amino coupling agent and the end-capping agent is (80-98): (1-5): (0.5-3).

3. The preparation method of amino silicone oil softener according to claim 1, It is characterized in that In the step (1), the end-capping agent includes at least one of hexamethyldisiloxane and octamethyltrisiloxane.

4. The preparation method of the amino silicone oil softener according to claim 1, It is characterized in that In the step (1), the alkaline catalyst includes at least one of potassium hydroxide and tetramethylammonium hydroxide.

5. The preparation method of amino silicone oil softener according to claim 1, It is characterized in that In the step (2), the organic solvent includes isopropanol.

6. The preparation method of the amino silicone oil softener according to claim 1, It is characterized in that In the step (2), the mass ratio of the aminosilicone oil intermediate to the quaternary ammonium agent and the organic solvent is (60-80):(4-6):(20-30).

7. The preparation method of the amino silicone oil softener according to claim 1, It is characterized in that In the step (3), the mass ratio of the quaternary ammonium modified amino silicone oil to the emulsifier is (1-4):

1.

8. The amino silicone oil softener prepared by the preparation method of the amino silicone oil softener according to any one of claims 1 to 7.

9. Use of the amino silicone oil softener according to claim 8 in fabric finishing.