A method for preparing asphalt mixture warm mix agent using urban sewage sludge
By performing alkali melting reaction and hydrothermal treatment of urban sludge incineration ash with sodium hydroxide powder, zeolites with high Si/Al ratio and small particle size were prepared as a warm mixing agent for asphalt mixture, foamed asphalt was solved The high cost of mixing agent for mixing and difficulty in sludge utilization have been achieved, and low-cost and low-energy consumption of asphalt mixture preparation and sludge resource utilization have been achieved.
Patent Information
- Application Number
- CN202410259642.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-03-07
AI Technical Summary
In the prior art, the hot mixing agent for foamed asphalt mixture is high, and the particle size of urban domestic sludge incineration ash is small and light, making it difficult to effectively utilize, resulting in increased environmental pollution and production costs after sludge incineration.
The urban sludge incineration ash with sodium hydroxide powder was carried out to form a crystalline gel, and the synthetic zeolite was prepared by hydrothermal reaction and crystallization filtration steps, as a warm mixing agent for the asphalt mixture, and the moles of Si and Al were adjusted. To improve output and properties.
It effectively reduces the preparation cost of the asphalt mixture warm mixing agent, improves the foaming effect, reduces the mixing and paving temperature, improves the overall performance of the asphalt mixture, and realizes the resource utilization of sludge.
Smart Images

Figure CN118027520B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt mixture, in particular to a method for preparing asphalt mixture warm mix agent by utilizing urban sludge. Background Art
[0002] Municipal domestic sludge is a byproduct of sewage treatment. In my country, landfill is the main method of disposing sludge incineration ash. Zero landfill resource utilization has become the research focus of sludge incineration technology. However, the current resource utilization of sludge incineration ash is limited by the market's consumption capacity, and in actual operation it cannot fully meet the demand for sludge incineration capacity.
[0003] Compared with traditional hot-mix asphalt pavement, warm-mix asphalt mixture can reduce the construction temperature of asphalt pavement, significantly reduce energy consumption and carbon dioxide emissions, and will not have a negative impact on engineering performance. Asphalt foaming is a warm-mix technology that temporarily improves the workability of asphalt mixture by adding water. Among them, synthetic zeolite is the most widely used foaming asphalt mixture warm-mix agent. There are large cavities and pores in the structure of zeolite, which can lose water without damaging the crystal structure. The crystal water in the zeolite structure can be removed by heating or other methods, and can be used as a carrier for other liquids besides water. During the mixing process of the mixture, the asphalt mixture warm-mix aid is added at the same time as the heated asphalt. The large amount of steam generated by the warm-mix aid containing crystal water will cause the asphalt volume to expand to form foamed asphalt, which can significantly reduce the mixing and compaction temperature of the asphalt mixture, and can effectively reduce exhaust emissions and energy consumption.
[0004] However, synthetic zeolite is usually prepared by hydrothermal synthesis of sodium silicate aqueous solution and sodium aluminate aqueous solution, which leads to high cost and increases the production cost of asphalt mixture. The price of foaming asphalt mixture warm mix agent commonly used in engineering practice is relatively high, which increases the production cost of asphalt mixture to a certain extent, and the reduced energy consumption can only compensate for part of the production cost. At the same time, the ash from the incineration of urban domestic sludge has a small particle size and light weight, and its main components are silicates, phosphates, metal particles and oxides. Therefore, how to use the ash from the incineration of urban domestic sludge to synthesize zeolite to reduce production costs is a technical problem that needs to be solved by the present invention. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a warm mix agent for asphalt mixture using urban sludge. By using artificially synthesized zeolite from urban sludge as a warm mix agent for asphalt mixture, the problem of multi-faceted pollution to the environment caused by incineration of urban sludge is solved, and the problem of high cost of foamed asphalt mixture warm mix agent in the prior art is solved.
[0006] To achieve the above object, the present invention provides a method for preparing asphalt mixture warm mix agent using municipal sludge, comprising the following steps:
[0007] (1) Alkali melting stage: the municipal sewage sludge incineration ash and sodium hydroxide powder are mixed evenly and placed in a ceramic crucible for calcination to obtain a molten product;
[0008] (2) hydrothermal reaction stage: the molten product obtained in (1) is mixed evenly with a sodium hydroxide solution to obtain a mixed solution, the supernatant is extracted by filtration, and sodium aluminate powder is added to adjust the molar ratio of Si and Al to form a crystalline gel;
[0009] (3) Crystallization and filtration stage: The crystallized gel obtained in (2) is transferred into a polytetrafluoroethylene container for crystallization, and the synthetic product is separated by filtration after rapid cooling, and the synthetic asphalt mixture warm mix agent is obtained after washing and drying.
[0010] Preferably, (1) in the alkali melting stage, the mass ratio of municipal sewage sludge incineration ash to sodium hydroxide powder is 0.8-1.25, the ceramic crucible is calcined at a temperature of 500-600°C, and heated in air for 1 hour. The present invention uses an X-ray diffractometer (XRD) to perform crystal phase analysis on the molten product, compares the soluble silicate content at different mass ratios of sewage sludge incineration ash to sodium hydroxide powder, and determines that the mass ratio of sewage sludge incineration ash to sodium hydroxide powder with the highest soluble aluminosilicate content is the optimal mass ratio.
[0011] The crystalline quartz (SiO2) in the municipal sewage sludge incineration ash used in the present invention is converted into silicate by alkaline melting. The present invention maximizes the conversion rate of the crystalline quartz (SiO2) in the municipal sewage sludge incineration ash by controlling the mass ratio of the municipal sewage sludge incineration ash to the sodium hydroxide powder within the above-mentioned range, thereby increasing the output of the final asphalt mixture warm mix agent and saving the raw material sodium hydroxide powder.
[0012] The present invention controls the calcining time of the ceramic crucible within the above range, so that the crystalline phase in the municipal sludge incineration ash is completely transformed, while also avoiding the situation that the calcining time is too short, which will lead to incomplete melting reaction and incomplete destruction of the crystal structure in the municipal sludge incineration ash; and the calcining time is too long, which will consume too much energy.
[0013] Preferably, in the (2) hydrothermal reaction stage, the solid-liquid ratio of the molten product to the sodium hydroxide solution is 1:10 g / ml, and the mixture is mixed at a temperature of 65° C. by stirring with a magnetic stirrer for 3 hours.
[0014] In the hydrothermal reaction stage, Si and Al in the molten product need to be dissolved in the solution. If the solubility of Si and Al is limited, the amount of the synthesized product will be very small. In the present invention, the molten product and the sodium hydroxide solution are controlled within the above range to ensure that Si and Al in the molten product can be fully dissolved in the solution, thereby increasing the output of the final asphalt mixture warm mix agent.
[0015] Preferably, the concentration of the sodium hydroxide solution is 1 to 3 mol / L. The present invention can fully dissolve Si and Al in the molten product by controlling the concentration of the sodium hydroxide solution within the above range.
[0016] Preferably, in (2) the hydrothermal reaction stage, since the undissolved solid impurities seriously affect the subsequent hydrothermal crystallization reaction, the mixed solution is filtered and the supernatant is extracted, and the Si and Al concentrations in the supernatant are analyzed by inductively coupled plasma optical emission spectroscopy, and then sodium aluminate powder is added to adjust the molar ratio of Si to Al in the supernatant to 0.75 to 0.85. The present invention adjusts the molar ratio of Si to Al in the supernatant, thereby facilitating the control of the output of the synthetic product and the properties of the synthetic product, such as the crystal water content and the crystal water release rate.
[0017] Preferably, in the (3) crystallization and filtration stage, the crystallization temperature is 80° C. and the crystallization reaction time is 3 hours.
[0018] Preferably, the synthetic product separated by filtration in the crystallization filtration stage (3) is repeatedly washed with distilled water and then dried at 60° C. for 12 hours. The crystallization water release of the synthetic asphalt mixture warm mix is calculated using a thermogravimetric differential thermal analyzer.
[0019] Beneficial effects of the present invention:
[0020] 1. The present invention adopts the incineration ash of urban domestic sludge to make artificial synthetic zeolite, which is used as a warm mix agent for asphalt mixture, which can effectively reduce the preparation cost of the warm mix agent for asphalt mixture, and at the same time provide an efficient solution for the reasonable disposal and resource utilization of urban domestic sludge.
[0021] 2. The asphalt mixture warm mix prepared by the present invention has a water content of up to about 20%, and has a higher Si / Al ratio, more divalent cations and a smaller particle size, so that it has a stronger water binding force, and can release water more slowly during the preparation of the asphalt mixture, resulting in a better foaming effect.
[0022] 3. The asphalt mixture warm mix agent prepared by the present invention can gradually release about 20% of crystal water from 70°C to 200°C, which can effectively reduce the mixing and paving temperature of the asphalt mixture by 25°C.
[0023] 4. It can be seen from the embodiments and comparative examples of the present invention that the overall performance of the warm-mix asphalt mixture prepared by the asphalt mixture warm-mix agent prepared by the present invention is better than that of the warm-mix asphalt mixture added with commercial warm-mix agent, and is comparable to the overall performance of the traditional hot-mix mixture.
[0024] 5. The asphalt mixture warm mix agent prepared by the present invention is an economical and efficient warm mix agent that can produce significant economic, social and ecological benefits.
[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a flow chart of a method for preparing asphalt mixture warm mix agent by utilizing urban sewage sludge. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0028] The municipal sludge incineration ash used in the present invention is obtained from a sewage treatment plant, and its main chemical components are analyzed using X-ray fluorescence spectroscopy, as shown in the following Table 1.
[0029] Table 1 Chemical composition of sludge incineration ash extracted from sewage treatment plants
[0030]
[0031] Example 1
[0032] Figure 1 The flowchart of the method for preparing asphalt mixture warm mix agent by using urban sludge of the present invention is as shown in the figure. The method for preparing asphalt mixture warm mix agent by using urban sludge provided by the present invention comprises the following steps:
[0033] (1) 1000 g of incineration ash and 1150 g of sodium hydroxide powder were weighed and placed in a ceramic crucible and mixed evenly, and then placed in a muffle furnace and calcined at 600° C. for 1 hour to activate the sludge incineration ash through an alkaline melting reaction;
[0034] (2) dissolving the molten product in a sodium hydroxide solution with a concentration of 2.5 mol / L at 65° C., with a solid-liquid ratio of the molten product to the sodium hydroxide solution of 1:10 g / ml, stirring the mixture at 500 rpm for 3 hours using a magnetic stirrer to ensure that the solution is uniformly mixed, filtering the mixed solution, extracting the supernatant and adding sodium aluminate powder, mixing the mixture uniformly using a magnetic stirrer, and adjusting the Si / Al molar ratio in the solution to 0.8 to form a crystalline gel;
[0035] (3) The crystallized gel obtained in (2) is transferred into a polytetrafluoroethylene container, and the reaction container is transferred into a water bath container at 80° C. to rapidly cool and crystallize, the synthetic product is separated by filtration and repeatedly washed with distilled water, and then dried in an oven at 60° C. for 12 hours to obtain a synthetic product; the product is fully ground to obtain an asphalt mixture warm mix agent.
[0036] Example 2
[0037] The present invention provides a method for preparing a warm mix asphalt mixture by using municipal sludge, comprising the following steps:
[0038] (1) 1000 g of incineration ash and 1250 g of sodium hydroxide powder were weighed and placed in a ceramic crucible and mixed evenly, and then placed in a muffle furnace and calcined at 500° C. for 1 hour to activate the sludge incineration ash through an alkaline melting reaction;
[0039] (2) dissolving the molten product in a sodium hydroxide solution with a concentration of 1 mol / L at 65° C., with a solid-liquid ratio of the molten product to the sodium hydroxide solution of 1:10 g / ml, stirring the mixture at 500 rpm for 3 hours using a magnetic stirrer to ensure that the solution is uniformly mixed, filtering the mixed solution, extracting the supernatant and adding sodium aluminate powder, mixing the mixture uniformly using a magnetic stirrer, and adjusting the Si / Al molar ratio in the solution to 0.75 to form a crystalline gel;
[0040] (3) The crystallized gel obtained in (2) is transferred into a polytetrafluoroethylene container, and the reaction container is transferred into a water bath container at 80° C. to rapidly cool and crystallize, the synthetic product is separated by filtration and repeatedly washed with distilled water, and then dried in an oven at 60° C. for 12 hours to obtain a synthetic product; the product is fully ground to obtain an asphalt mixture warm mix agent.
[0041] Example 3
[0042] The present invention provides a method for preparing a warm mix asphalt mixture by using municipal sludge, comprising the following steps:
[0043] (1) 1000 g of incineration ash and 800 g of sodium hydroxide powder were weighed and placed in a ceramic crucible and mixed evenly, and then placed in a muffle furnace and calcined at 550° C. for 1 hour to activate the sludge incineration ash through an alkaline melting reaction;
[0044] (2) dissolving the molten product in a 3 mol / L sodium hydroxide solution at 65° C., with a solid-liquid ratio of the molten product to the sodium hydroxide solution of 1:10 g / ml, stirring the mixture at 500 rpm for 3 hours using a magnetic stirrer to ensure that the solution is uniformly mixed, filtering the mixed solution, extracting the supernatant and adding sodium aluminate powder, mixing the mixture uniformly using a magnetic stirrer, and adjusting the Si / Al molar ratio in the solution to 0.85 to form a crystalline gel;
[0045] (3) The crystallized gel obtained in (2) is transferred into a polytetrafluoroethylene container, and the reaction container is transferred into a water bath container at 80° C. to rapidly cool and crystallize, the synthetic product is separated by filtration and repeatedly washed with distilled water, and then dried in an oven at 60° C. for 12 hours to obtain a synthetic product; the product is fully ground to obtain an asphalt mixture warm mix agent.
[0046] Performance Testing
[0047] The crystal water content of the asphalt mixture warm mix prepared in Example 1 was calculated to be 18.57% by using a thermogravimetric differential thermal analyzer.
[0048] The asphalt mixture warm mix agent prepared in Example 1 of the present invention is used to prepare a conventional hot mix asphalt mixture, the stone used is granite, the grading is SMA10, the asphalt is SBS modified asphalt (PG76-16), the asphalt dosage is 6.0%, the fiber dosage is 0.3%, and the asphalt warm mix agent dosage is 0.3%. At the same time, a commercial warm mix agent is used to prepare a warm mix asphalt mixture and a hot mix asphalt mixture for comparison. The prepared asphalt mixture is subjected to a performance test, and the test results are shown in Table 2.
[0049] Table 2 Asphalt mixture performance test results
[0050]
[0051] In order to evaluate the cost-effectiveness of the asphalt mixture warm mix agent prepared by the present invention, a cost-effectiveness quantitative analysis was conducted on its synthesis process and asphalt mixture preparation process, and the results are shown in Table 3. In the cost-effectiveness analysis, the cost mainly includes the input material and energy costs, and the benefit mainly includes the income brought by the by-products in the synthesis process. Since the cost of the asphalt mixture warm mix agent prepared in Example 1 of the present invention is calculated based on the market price and energy consumption of the raw materials collected under laboratory conditions, the cost is expected to be reduced under market-oriented large-scale production.
[0052] Table 3 Cost-effectiveness analysis
[0053] Warm mix type Example 1 Warm mix agent Commercial warm mix Cost (yuan / kg) 6.26 9.71 Benefit (yuan / kg) 0.51 0
[0054] In summary, the asphalt mixture warm mix agent provided by the present invention can significantly reduce the mixing temperature of asphalt and aggregate and the molding temperature under the premise of achieving the same compaction effect, and the temperature reduction range reaches 25°C. At the same time, the overall engineering performance of the prepared warm mix asphalt mixture is similar to that of the hot mix asphalt mixture, and is superior to the warm mix asphalt mixture containing commercial foaming additives in terms of crack resistance, fatigue resistance and water damage resistance.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing asphalt mixture warm mix agent using municipal sludge, characterized in that: The following steps are involved: (1) Alkali melting stage: the municipal sewage sludge incineration ash and sodium hydroxide powder are mixed evenly and placed in a ceramic crucible for calcination to obtain a molten product; The mass ratio of municipal sewage sludge incineration ash to sodium hydroxide powder is 0.8-1.25, the ceramic crucible is calcined at a temperature of 500-600°C, and heated in air for 1 hour; (2) hydrothermal reaction stage: the molten product obtained in (1) is mixed evenly with a sodium hydroxide solution to obtain a mixed solution, the supernatant is extracted by filtration, and sodium aluminate powder is added to adjust the molar ratio of Si and Al to form a crystalline gel; (3) Crystallization and filtration stage: the crystallized gel obtained in (2) is transferred into a polytetrafluoroethylene container for crystallization, and the synthetic product is separated by filtration after rapid cooling, and the synthetic asphalt mixture warm mix agent is obtained after washing and drying; Asphalt warm mix agent is used to prepare asphalt mixture.
2. The method for preparing asphalt mixture warm mix agent using municipal sludge according to claim 1, characterized in that: (2) In the hydrothermal reaction stage, the molten product was mixed with a sodium hydroxide solution at a solid-to-liquid ratio of 1:10 g / ml at a temperature of 65° C. and the mixing method was stirring with a magnetic stirrer for 3 hours.
3. The method for preparing asphalt mixture warm mix agent using municipal sludge according to claim 2, characterized in that: The concentration of the sodium hydroxide solution is 1 to 3 mol / L.
4. The method for preparing asphalt mixture warm mix agent using municipal sludge according to claim 1, characterized in that: (2) During the hydrothermal reaction stage, after filtering the mixed solution, the Si and Al concentrations in the supernatant were analyzed using inductively coupled plasma optical emission spectroscopy, and sodium aluminate powder was added to adjust the molar ratio of Si to Al in the supernatant to 0.75-0.
85.
5. The method for preparing asphalt mixture warm mix agent using municipal sludge according to claim 1, characterized in that: (3) In the crystallization and filtration stage, the crystallization temperature is 80°C and the crystallization reaction time is 3 hours.
6. The method for preparing asphalt mixture warm mix agent using municipal sludge according to claim 1, characterized in that: (3) The synthetic product separated by filtration in the crystallization filtration stage was repeatedly washed with distilled water and then dried at 60° C. for 12 hours.