A catalyst and a preparation method thereof and a method for catalytically hydrogenating SiCl4 to produce SiHCl3

By uniformly loading the multi-stage pore structure catalyst of precious metals and transition metals on the ZSM-5 molecular sieve support, the problem of low conversion of silicon tetrachloride is solved, and efficient SiHCl3 production is achieved, reducing energy consumption and investment, and is suitable for industrial applications. .

CN118045626BActive Publication Date: 2024-11-08WUHUAN ENG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311788817.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-11-08
Estimated Expiration
2043-12-25

AI Technical Summary

Technical Problem

In the prior art, the recovery conversion rate of silicon tetrachloride is low, resulting in waste of silicon resources and environmental pollution. The thermal hydrogenation method and cold hydrogenation method have high energy consumption, large investment, and low catalyst selectivity and yield.

Method used

The catalyst was prepared by co-precipitation method by using a ternary multi-stage pore structure catalyst, including alkali-modified ZSM-5 sodium-free silicon-aluminum molecular sieve support and uniformly supported precious metals, transition metals and Group II metals, and used to catalyze the hydrogenation of SiCl4 to produce SiHCl3. The addition of silicon powder and high temperature and high pressure conditions are avoided, and the active site and dispersion of the catalyst are improved.

Benefits of technology

At lower temperatures and pressures, the silicon tetrachloride conversion rate of the catalyst reaches 98.9%, and the single-way selectivity of trichlorosilicon is as high as 21-22%, reducing the reaction energy consumption and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004625845050000071
    Figure BDA0004625845050000071
Patent Text Reader

Abstract

The present invention discloses a catalyst and a preparation method thereof and a method for catalytically hydrogenating SiCl4 to produce SiHCl3. The catalyst is a ternary multi-level pore structure catalyst, including a carrier and an active metal uniformly loaded on the carrier; the carrier is an alkali-modified ZSM-5 sodium-free silicon-aluminum molecular sieve; the active metal includes a noble metal, a transition metal and a Group II metal. The present invention adopts a multi-level pore structure carrier to load a variety of active metals to make a hydrogenation catalyst, which can effectively disperse active metal particles, increase the specific surface area and the number of active sites of the catalyst, so that the thermal hydrogenation reaction can still produce SiHCl3 with high selectivity at a lower temperature, and improve the hydrogenation efficiency compared to the traditional thermal hydrogenation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recovering trichlorosilane from hydrogenated silicon tetrachloride, and specifically relates to a catalyst and a preparation method thereof and a method for catalytically hydrogenating SiCl4 to produce SiHCl3. Background Art

[0002] In the modified Siemens process for polysilicon production, which is currently used in most domestic processes, SiCl4 is generated during the synthesis and reduction stages of SiHCl3. Every 10,000 tons of polysilicon produced will produce 200,000 tons of SiCl4. If this part of SiCl4 is not utilized, it will not only cause serious environmental pollution, but also cause a large amount of silicon resources to be wasted. The main methods for recovering silicon tetrachloride in industry are thermal hydrogenation and cold hydrogenation. The thermal hydrogenation method is the reaction of silicon tetrachloride and hydrogen at high temperature (900-1100°C) without a catalyst to prepare trichlorosilane, which is currently one of the important methods for processing silicon tetrachloride. The single-pass conversion rate of silicon tetrachloride by the thermal hydrogenation method is 17-20%, with high operating energy consumption, large investment, and low conversion rate. Correspondingly, the yield of SiHCl3 is low.

[0003] The main reaction equation is as follows:

[0004] SiCl4+H2→SiHCl3+HCl

[0005] The main principle of cold hydrogenation technology is to use iron-based or copper-based catalysts to add silicon powder and hydrogen to the fluidized bed at 500-600°C, and react them with SiCl4 to produce SiHCl3. The conversion rate of cold hydrogenation SiCl4 is 25-35%, but silicon powder needs to be added during the reaction and by-products such as SiH2C12 and high-boiling silicon polymers will be produced. In industrial equipment, since the addition of silicon powder causes greater wear on the equipment, the material requirements for the equipment are relatively high, and the equipment investment is relatively large. The reaction equation is as follows:

[0006] Si+2H2+3SiCl4→4SiHCl3(main reaction)

[0007] Si+2H2+SiCl4→2SiH2Cl2(side reaction)

[0008] 2SiHCl3ρSiH2+2SiCl4(side reaction)

[0009] In order to improve the yield of trichlorosilane and reduce the reaction energy consumption, Chinese invention patent CN104399479A discloses a copper-lanthanum co-impregnated silicon-based catalyst. Under the conditions of 450°C and 1MPa, the conversion rate of silicon tetrachloride reaches 30.17%, and the selectivity of trichlorosilane is 100%. However, silicon powder needs to be added during the reaction. Chinese invention patent CN103007995A discloses a catalyst in which a transition metal and a group II metal are co-impregnated on a porous carrier. The catalyst can smooth the reaction conditions of thermal hydrogenation. Under the conditions of 750-950°C, the single-pass conversion rate of SiCl4 can reach 20-26.62%, but the selectivity of SiHCl3 is not high, and the yield is only 16-19%. Summary of the invention

[0010] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a catalyst with good formability, high strength, good activity and stable performance and a preparation method thereof, and a method for catalytically hydrogenating SiCl4 to produce SiHCl3.

[0011] To achieve the above-mentioned purpose, the present invention provides a catalyst for catalytic hydrogenation of SiCl4 to produce SiHCl3, wherein the catalyst is a ternary multi-level pore structure catalyst, comprising a carrier and an active metal uniformly loaded on the carrier; the carrier is an alkali-modified ZSM-5 sodium-free silicon-aluminum molecular sieve, wherein the mass fraction ratio of SiO2 / Al2O3 is 100:1 to 350:1; the active metal comprises a noble metal, a transition metal and a Group II metal, wherein the mass of the noble metal is 0.1 to 1% of the mass of the carrier, the mass of the transition metal is 2 to 10% of the mass of the carrier, and the mass of the Group II metal is 5 to 15% of the mass of the carrier.

[0012] Furthermore, the noble metal is Pt, the transition metal is any one of Ni, Cu, Co, Ce or La (preferably Ni, Ce or Co), and the Group II metal is any one of Mg, Ca or Ba (preferably Mg or Ba).

[0013] A method for preparing the catalyst as described above is also provided, and the preparation method is as follows:

[0014] 1) Precious metals, transition metals and Group II metals are respectively prepared into precursor solutions and mixed into a mixed metal precursor solution; alkali-modified ZSM-5 sodium-free silicon-alumina molecular sieve is prepared into an alkali-modified ZSM-5 sodium-free silicon-alumina molecular sieve suspension;

[0015] 2) uniformly dropping the first alkaline solution and the mixed metal precursor solution into the alkali-modified ZSM-5 sodium-free silica-alumina molecular sieve suspension at 50-80° C., and stirring evenly to make the pH of the mixed solution be 7-7.5;

[0016] 3) Aging, centrifugal washing, drying and calcining to obtain a ternary multi-level pore structure catalyst.

[0017] Furthermore, in the step 1), the alkali-modified ZSM-5 sodium-free silica-alumina molecular sieve is prepared by alkali modification of the ZSM-5 molecular sieve, and the specific process is: the ZSM-5 molecular sieve is made into a ZSM-5 molecular sieve suspension, the second alkali solution is uniformly added to the ZSM-5 molecular sieve suspension, and after uniform stirring, the alkali-modified ZSM-5 molecular sieve is obtained after crystallization, centrifugal washing, drying, and calcination.

[0018] Furthermore, the mass concentration of the ZSM-5 molecular sieve suspension is 20-50 g / L, the molar concentration of the second alkaline solution is 0.01-2 mol / L (preferably 0.05-1 mol / L), the dripping rate is 2.3-6.7 ml / min; the crystallization temperature is 160-180° C., the crystallization time is 24-48 h, the calcination temperature is 450-600° C., the calcination time is 2-4 h and then taken out.

[0019] Furthermore, the specific surface area of ​​the ZSM-5 molecular sieve is 150 to 200 m 2 / g, a diameter of 3 to 5 mm; the specific surface area of ​​the alkali-modified ZSM-5 molecular sieve is 250 to 400 m 2 / g, pore diameter is 30-50nm.

[0020] Furthermore, in the step 1), the noble metal precursor solution, the transition metal precursor solution and the Group II metal precursor solution are all any one of nitrate solution, chloride solution, sulfate solution or acetate solution (preferably nitrate solution); the first alkaline solution is any one of sodium hydroxide, sodium carbonate or ammonia water (preferably sodium carbonate), and the molar concentration of the first alkaline solution is 0.1 to 1 mol / L; the second alkaline solution is any one of sodium carbonate, sodium hydroxide, tetramethylammonium hydroxide, tetrapropylammonium hydroxide or dimethyldiethylammonium hydroxide (preferably tetramethylammonium hydroxide, tetrapropylammonium hydroxide or dimethyldiethylammonium hydroxide organic base).

[0021] Furthermore, in the step 3), the aging time is 2 to 12 hours, the aging temperature is 50 to 80° C., the drying temperature is 90 to 110° C., the calcination temperature is 350 to 500° C., and the calcination time is 2 to 4 hours.

[0022] Finally, a method for producing SiHCl3 by catalytic hydrogenation of SiCl4 using the above catalyst is provided, wherein:

[0023] Before the reaction, an inert gas is introduced to purge the entire reaction system. The catalyst is loaded into the bed of the reaction system. Before the first use, H2 is introduced for heating pre-reduction. The pre-reduction temperature is 400-800°C, the heating rate is 1-3°C / min, the pre-reduction time is 4-24h, and the H2 flow rate is 20-120ml / min.

[0024] The reaction raw materials SiCl4 and H2 are preheated to 80-180°C and then contact the catalyst in the bed to react. The reaction temperature is 750-950°C, the reaction pressure is 0.5-3.5MPa, and the reaction time is 2.5-7.5h.

[0025] Furthermore, the H2 / SiCl4 molar ratio is 1:1-10, and the reaction space velocity is 200-1200h -1 .

[0026] The present invention adopts a coprecipitation method to prepare a ternary multi-level pore structure catalyst, and the active metal is uniformly loaded on the surface and inside of the molecular sieve with high specific surface area modified by alkali. Through the multi-level pore loading, metal agglomeration can be avoided, the number of active sites is increased, the efficiency of hydrogenation reaction is improved, and the reaction energy barrier is effectively reduced. Compared with the bifunctional catalyst prepared by the conventional impregnation method, the active metal particles formed by the catalyst have smaller particle size and more uniform dispersion. At a lower temperature (750-950°C) and pressure (0.5-3.5MPa), silicon tetrachloride can be catalyzed to convert into trichlorosilane without adding silicon powder. The single-pass selectivity of trichlorosilane is as high as 98.9%, and the yield can reach 21-22%.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1) The present invention adopts a multi-level pore structure carrier to load a variety of active metals to prepare a hydrogenation catalyst, which can effectively disperse the active metal particles, increase the specific surface area and the number of active sites of the catalyst, and improve the efficiency of the hydrogenation reaction.

[0029] 2) Compared with the thermal hydrogenation reaction, the catalyst of the present invention can catalyze the conversion of silicon tetrachloride to trichlorosilane at a lower temperature (750-950°C) and pressure (0.5-3.5MPa) without the addition of silicon powder, and the single-pass selectivity of trichlorosilane is as high as 98.9%, and the yield can reach 21-22%.

[0030] 3) The method for producing trichlorosilane by catalytic hydrogenation of silicon tetrachloride of the present invention has a simple process, can be carried out at a relatively low temperature, and is suitable for industrial production. DETAILED DESCRIPTION

[0031] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with examples. The salts used in the comparative examples and examples are calculated with a purity of >99.5%.

[0032] Example 1

[0033] 1) Preparation of ternary multi-level pore structure catalyst: 2 g of ZSM-5 molecular sieve was placed in 100 mL of deionized water to obtain solution A, wherein the mass ratio of Al2O3 / SiO2 was 150:1; 100 ml of 0.2 mol / L tetrapropylammonium hydroxide solution was prepared to obtain solution B, and solution B was added dropwise to solution A at a rate of 5 ml / min, and stirred evenly for 30 min; the mixed solution was then transferred to a reactor, reacted at 170°C for 24 h, taken out, centrifuged for cleaning, dried, and calcined at 550°C for 4 h to obtain an alkali-modified ZSM-5 molecular sieve.

[0034] Take 10g of alkali-modified ZSM-5 molecular sieve and place it in 100ml of deionized water to make solution C, prepare 80ml of 1.04mol / LNa2CO3 solution D, and then dissolve 0.042gH2PtCl6, 0.559gNi(NO3)2·9H2O, and 0.954gBa(NO3)2 in 80ml of water to make solution E; slowly add solution D and solution E to solution C at 80℃ at the same time, stir evenly, and keep the pH of the mixed solution between 7 and 7.5; after stirring at 80℃ for 30min, continue to age for 12h, and then the mixed solution is centrifugally washed and calcined at 400℃ for 4h to obtain a co-precipitated ternary multi-level pore structure catalyst, recorded as cat-1.

[0035] 2) Hydrogenation of silicon tetrachloride: Fill the reaction tube with the ternary multi-level porous structure catalyst cat-1, purge it with nitrogen three times, introduce hydrogen to reduce the catalyst, heat the reaction tube at a heating rate of 2°C / min to 550°C, and reduce it for 12h, wherein the flow rate of hydrogen is 50ml / min; after the reduction reaction is completed, the temperature continues to rise to 750°C and the pressure rises to 3MPa, the gasifier is preheated to 100°C, SiCl4 and H2 are introduced, and the two are mixed evenly in the gasifier and enter the reaction tube, contact the catalyst bed, and start the reaction, and the reaction space velocity is 1000h -1 , H2 / SiCl4 molar ratio is 5, and the reaction time is 4-7 hours. After condensation and gas-liquid separation, the product is analyzed by online GC-MS for the content of SiHCl3 and SiCl4. The results are shown in Table 1.

[0036] Example 2

[0037] 1) Preparation of ternary multi-level porous structure catalyst: In this embodiment, the transition metal precursor is Ce(NO3)3·6H2O, and the addition amount is 0.620g, and the group II metal precursor is Mg(NO3)2·6H2O, and the addition amount is 5.275g. The rest of the preparation method is consistent with that in Example 1. The co-precipitated ternary multi-level porous structure catalyst is recorded as cat-2.

[0038] 2) Hydrosilane tetrachloride reaction: The pre-reduction step of the catalyst in this embodiment is consistent with that in Example 1, and the remaining conditions and reaction steps are consistent with those in Example 1.

[0039] Example 3

[0040] 1) Preparation of ternary multi-level porous structure catalyst: In this embodiment, the transition metal precursor is La(NO3)3·6H2O, and the addition amount is 0.623g. The group II metal precursor is Ba(NO3)2, and the addition amount is 0.954g. The rest of the preparation method is consistent with Example 1. The co-precipitated ternary multi-level porous structure catalyst is recorded as cat-3.

[0041] 2) Hydrosilane tetrachloride reaction: The pre-reduction step of the catalyst in this embodiment is consistent with that in Example 1, and the remaining conditions and reaction steps are consistent with those in Example 1.

[0042] Example 4

[0043] 1) Preparation of ternary multi-level porous structure catalyst: In this embodiment, the transition metal precursor is Cu(NO3)2·6H2O, and the addition amount is 0.755g, and the group II metal precursor is Sr(NO3)2, and the addition amount is 1.208g. The rest of the preparation method is consistent with that in Example 1. The co-precipitated ternary multi-level porous structure catalyst is recorded as cat-4.

[0044] 2) Hydrosilane tetrachloride reaction: The catalyst pre-reduction step in this example is the same as that in Example 1, but the reaction temperature is 850° C. and the reaction pressure is 1 MPa. The remaining conditions and reaction steps are the same as those in Example 1.

[0045] Example 5

[0046] 1) Preparation of ternary multi-level porous structure catalyst: In this embodiment, the transition metal precursor is Co(NO3)2·6H2O, and the addition amount is 0.988g, and the group II metal precursor is Ba(NO3)2, and the addition amount is 0.954g. The rest of the preparation method is consistent with that in Example 1. The co-precipitated ternary multi-level porous structure catalyst is recorded as cat-5.

[0047] 2) Hydrosilane tetrachloride reaction: The pre-reduction step of the catalyst in this embodiment is consistent with that in embodiment 1, but the reaction temperature is 950° C., and the other conditions and reaction steps are consistent with those in embodiment 1.

[0048] Example 6

[0049] 1) Preparation of ternary multi-level pore structure catalyst: The preparation method of the catalyst in this example is consistent with that in Example 1. The co-precipitated ternary multi-level pore structure catalyst obtained is recorded as cat-6.

[0050] 2) Hydrosilane tetrachloride reaction: The pre-reduction step of the catalyst in this embodiment is consistent with that in Example 1, but the reaction temperature is 850° C., the reaction pressure is 3.3 MPa, and the other conditions and reaction steps are consistent with those in Example 1.

[0051] Example 7

[0052] 1) Preparation of ternary multi-level pore structure catalyst: The preparation method of the catalyst in this example is consistent with that in Example 1. The co-precipitated ternary multi-level pore structure catalyst obtained is recorded as cat-7.

[0053] 2) Hydrosilane tetrachloride reaction: The pre-reduction step of the catalyst in this embodiment is consistent with that in Example 1, but the reaction temperature is 950° C. and the reaction pressure is 3.3 MPa. The other conditions and reaction steps are consistent with those in Example 1.

[0054] Comparative Example 1

[0055] 1) Preparation of catalyst: Using the impregnation method disclosed in Chinese invention patent CN103007995A, 10g of alkali-modified ZSM-5 molecular sieve was impregnated in a mixed solution of H2PtCl6, Ni(NO3)2 and Ba(NO3)2, and the dosage of the three precursors was consistent with that in Example 1. During the 6h impregnation of equal volume, 100MHZ ultrasonic vibration was added to promote solution impregnation. After the impregnation was completed, the catalyst was taken out, dried at 150°C for 3h, and gradient calcined at 300-600°C for 6h to obtain a catalyst recorded as C-1.

[0056] 2) Hydrosilane tetrachloride reaction: The pre-reduction step of the catalyst in this embodiment is consistent with that in Example 1, the reactant temperature is 750° C., the reaction pressure is 3 MPa, and the remaining conditions and reaction steps are consistent with those in Example 1.

[0057] The results of catalyzing silicon tetrachloride to produce trichlorosilane in various embodiments and comparative examples are shown in Table 1.

[0058]

Claims

1. A method for catalytic hydrogenation of SiCl 4 Production of SiHCl 3 The catalyst Features: The catalyst is a ternary multi-level pore structure catalyst, comprising a carrier and an active metal uniformly loaded on the carrier; the carrier is an alkali-modified ZSM-5 sodium-free silicon-aluminum molecular sieve, wherein SiO 2 / Al 2 O 3 The mass ratio of the carrier is 100:1 to 350:1; the active metal includes a noble metal, a transition metal and a Group II metal, the mass of the noble metal is 0.1 to 1% of the mass of the carrier, the mass of the transition metal is 2 to 10% of the mass of the carrier, and the mass of the Group II metal is 5 to 15% of the mass of the carrier; the noble metal is Pt, the transition metal is any one of Ni, Cu, Co, Ce or La, and the Group II metal is any one of Mg, Ca or Ba; The preparation method of the catalyst is as follows: 1) Precious metals, transition metals and Group II metals are respectively prepared into precursor solutions and mixed into a mixed metal precursor solution; alkali-modified ZSM-5 sodium-free silicon-alumina molecular sieve is prepared into an alkali-modified ZSM-5 sodium-free silicon-alumina molecular sieve suspension; 2) uniformly dropping the first alkaline solution and the mixed metal precursor solution into the alkali-modified ZSM-5 sodium-free silica-alumina molecular sieve suspension at 50-80° C., and stirring evenly to make the pH of the mixed solution be 7-7.5; 3) Aging, centrifugal washing, drying and calcining to obtain a ternary multi-level pore structure catalyst.

2. A method for preparing the catalyst as claimed in claim 1, Features: The preparation method is as follows: 1) Precious metals, transition metals and Group II metals are respectively prepared into precursor solutions and mixed into a mixed metal precursor solution; alkali-modified ZSM-5 sodium-free silicon-alumina molecular sieve is prepared into an alkali-modified ZSM-5 sodium-free silicon-alumina molecular sieve suspension; 2) uniformly dropping the first alkaline solution and the mixed metal precursor solution into the alkali-modified ZSM-5 sodium-free silica-alumina molecular sieve suspension at 50-80° C., and stirring evenly to make the pH of the mixed solution be 7-7.5; 3) Aging, centrifugal washing, drying and calcining to obtain a ternary multi-level pore structure catalyst.

3. The method for preparing the catalyst according to claim 2, Features: In the step 1), the alkali-modified ZSM-5 sodium-free silica-alumina molecular sieve is prepared by alkali-modifying the ZSM-5 molecular sieve. The specific process is: the ZSM-5 molecular sieve is made into a ZSM-5 molecular sieve suspension, the second alkali solution is uniformly added to the ZSM-5 molecular sieve suspension, and the alkali-modified ZSM-5 molecular sieve is obtained after crystallization, centrifugal washing, drying, and calcination after stirring.

4. The method for preparing the catalyst according to claim 3, Features: The mass concentration of the ZSM-5 molecular sieve suspension is 20-50 g / L, the molar concentration of the second alkaline solution is 0.01-2 mol / L, and the dropping rate is 2.3-6.7 ml / min; the crystallization temperature is 160-180° C., the crystallization time is 24-48 h, the calcination temperature is 450-600° C., the calcination time is 2-4 h, and then it is taken out.

5. The method for preparing the catalyst according to claim 3, Features: The specific surface area of ​​the ZSM-5 molecular sieve is 150 to 200 m 2 / g, a diameter of 3 to 5 mm; the specific surface area of ​​the alkali-modified ZSM-5 molecular sieve is 250 to 400 m 2 / g, pore diameter is 30-50nm.

6. The method for preparing the catalyst according to claim 3, Features: In the step 1), the noble metal precursor solution, the transition metal precursor solution and the Group II metal precursor solution are all any one of nitrate solution, chloride solution, sulfate solution or acetate solution; the first alkaline solution is any one of sodium hydroxide, sodium carbonate or ammonia water, and the molar concentration of the first alkaline solution is 0.1-1 mol / L; the second alkaline solution is any one of sodium carbonate, sodium hydroxide, tetramethylammonium hydroxide, tetrapropylammonium hydroxide or dimethyldiethylammonium hydroxide.

7. The method for preparing the catalyst according to claim 2, Features: In the step 3), the aging time is 2 to 12 hours, the aging temperature is 50 to 80° C., the drying temperature is 90 to 110° C., the calcination temperature is 350 to 500° C., and the calcination time is 2 to 4 hours.

8. A catalyst for hydrogenating SiCl as claimed in claim 1 4 Production of SiHCl 3 method, Features: The method is: Before the reaction, the inert gas was introduced to purge the entire reaction system. The catalyst was loaded into the bed of the reaction system. H was introduced before the first use. 2 Heat pre-reduction, the pre-reduction temperature is 400-800°C, the heating rate is 1-3°C / min, the pre-reduction time is 4-24h, H 2 Flow rate 20~120ml / min; Reaction raw material SiCl 4 With H 2 After preheating to 80-180°C, the catalyst is contacted in the bed to react. The reaction temperature is 750-950°C, the reaction pressure is 0.5-3.5 MPa, and the reaction time is 2.5-7.5 hours.

9. Catalytic hydrogenation of SiCl by the catalyst according to claim 8 4 Production of SiHCl 3 method, Features: The H 2 / SiCl 4 The molar ratio is 1:1-10, and the reaction space velocity is 200-1200h -1 .