A high temperature resistant flexible deformable heat insulating wave absorbing material, skin and preparation method thereof

By using fiber matrix and airgel composite materials of silicon carbide fiber and oxide ceramic fiber in the thermal protection system, combined with origami structure and skin structure, the problem of traditional thermal insulation materials being unable to adapt to the shape change of high-speed variant aircraft is solved. It achieves improvements in large-scale deformation and stealth performance under high temperatures.

CN118046632BActive Publication Date: 2024-10-01BEIJING INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410159786.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2024-10-01
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

In traditional thermal protection systems, rigid ceramic insulation tiles are brittle and have poor mechanical properties, while flexible insulation blankets have poor followability and cannot adapt to the shape changes of high-speed morphing aircraft and cannot meet the high efficiency requirements of high-speed morphing aircraft. .

Method used

Provide a high-temperature-resistant, flexible and deformable heat-insulating and absorbing material that uses a fiber matrix composed of silicon carbide fiber and oxide ceramic fiber and is composited with aerogel. It uses an origami structure to achieve large-scale deformation, and is equipped with a skin structure, including anti-scouring layer, thermal insulation absorbing layer and gas barrier layer to improve the material's stealth and thermal insulation properties.

Benefits of technology

It achieves large-scale deformation under high and low temperature conditions, improves the stealth performance and fatigue resistance of thermal insulation materials, adapts to the multi-mission aerodynamic shape transformation of high-speed variant aircraft, and meets the aircraft's stealth performance requirements for thermal insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118046632B_ABST
    Figure CN118046632B_ABST
Patent Text Reader

Abstract

The present invention provides a high temperature resistant flexible deformable heat insulating absorbing material, a skin and a preparation method thereof, belonging to the technical field of heat insulating materials, wherein the deformable heat insulating absorbing material comprises a fiber matrix having an origami structure and a first aerogel reinforcement; the fiber matrix comprises a silicon carbide fiber layer and an oxide ceramic fiber layer. The deformable heat insulating material provided by the present invention has adjustable size and shape, can achieve large-scale deformation under both high and low temperature conditions, and has stealth performance, can adapt to the shape transformation of a variant aircraft, and meet the aircraft's requirements for stealth performance of heat insulating materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heat-insulating materials, and in particular to a high-temperature-resistant flexible and deformable heat-insulating and wave-absorbing material, a skin and a preparation method thereof. Background Art

[0002] The aerospace field is developing rapidly, and high-speed transformable aircraft have become a new trend for future development. During the launch and return of high-speed aircraft, a large amount of heat will be generated due to aerodynamic heating. In order to ensure the normal operation of the aircraft, a thermal protection system is usually used for protection. With the development of the aerospace and military industries, higher requirements are placed on the thermal protection system of aircraft. It is not only required to have excellent heat protection and heat insulation performance, but also to have good stealth and wave absorption performance. Traditional thermal protection systems include rigid ceramic insulation tiles and flexible insulation felts, but rigid insulation tiles are brittle and have poor mechanical properties, and flexible insulation felts have poor follow-up performance. They cannot adapt to the shape changes of transformable aircraft and cannot meet the high efficiency requirements of high-speed transformable aircraft.

[0003] Therefore, there is an urgent need to provide a thermal insulation material that can achieve large-scale deformation and has stealth properties. Summary of the invention

[0004] In response to one or more technical problems existing in the prior art, the present invention provides a high-temperature resistant flexible deformable heat-insulating and wave-absorbing material, a skin and a preparation method thereof. The deformable heat-insulating material provided by the present invention has adjustable size and shape, can achieve large-scale deformation under both high and low temperature conditions, and has stealth performance. It can adapt to the shape changes of variant aircraft and meet the aircraft's requirements for stealth performance of heat-insulating materials.

[0005] In a first aspect, the present invention provides a high temperature resistant flexible deformable heat insulating and absorbing material, wherein the deformable heat insulating and absorbing material comprises a fiber matrix having an origami structure and a first aerogel reinforcement.

[0006] The fiber matrix includes a silicon carbide fiber layer and an oxide ceramic fiber layer.

[0007] Preferably, the oxide ceramic fiber layer includes one or more of silica fiber, alumina fiber, and mullite fiber;

[0008] The thickness of the silicon carbide fiber layer is 0.5 to 1 mm; and / or

[0009] The thickness of the oxide ceramic fiber layer is 1 to 10 mm.

[0010] Preferably, the first aerogel reinforcement is one or more of silica aerogel, alumina aerogel, aluminum-silicon aerogel, SiOC aerogel, and SiOCN aerogel; preferably, the first aerogel reinforcement accounts for 30-60% of the total mass of the deformable thermal insulation and absorbing material.

[0011] Preferably, the origami structure is at least one of a Z-type origami structure, a Flasher origami structure, and a Miura origami structure.

[0012] In a second aspect, the present invention provides a method for preparing the deformable heat-insulating and wave-absorbing material according to the first aspect, the preparation method comprising the following steps:

[0013] Pre-treating and molding the fibers to obtain a fiber matrix;

[0014] The fiber matrix is ​​immersed in a first aerogel precursor impregnation liquid, and subjected to heat treatment, solvent replacement, and drying to obtain the deformable heat-insulating and wave-absorbing material.

[0015] Preferably, after the drying, pyrolysis is further included, and the pyrolysis temperature is 900-1200°C.

[0016] Preferably, the first aerogel precursor impregnation liquid comprises a first aerogel precursor, an organic solvent and a catalyst; preferably, the first aerogel precursor accounts for 20 to 50% of the total mass of the first aerogel precursor impregnation liquid;

[0017] Preferably, the first aerogel precursor is at least one of a silicon source and an aluminum source; more preferably, the silicon source is one or more of water glass, tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trimethylmethoxysilane, hexamethyldisilazane, and aminopropyltriethoxysilane; more preferably, the aluminum source is one or more of aluminum sec-butoxide, aluminum isopropoxide, aluminum chloride hexahydrate, and aluminum nitrate nonahydrate;

[0018] Preferably, the organic solvent is an alcohol, preferably one or more of methanol, ethanol, isopropanol and n-propanol;

[0019] Preferably, the catalyst is an acid solution or an alkaline solution, the acid solution is preferably one or more of hydrochloric acid, acetic acid and nitric acid; the alkaline solution is preferably one or more of ammonia water and sodium hydroxide solution; more preferably, the concentrations of the acid solution and the alkaline solution are independently 0.3 to 0.6 mol / L.

[0020] Preferably, the forming includes at least one of press forming, extrusion forming, and semi-manual folding forming;

[0021] The heat treatment temperature is 30-60°C; and / or

[0022] The drying method is at least one of normal pressure drying and supercritical drying.

[0023] The present invention provides a skin in a third aspect, the skin comprising an anti-scour layer, a heat-insulating and wave-absorbing layer and a gas-barrier layer arranged in sequence from the outside to the inside, the heat-insulating and wave-absorbing layer being the deformable heat-insulating and wave-absorbing material described in the first aspect.

[0024] Preferably, the anti-scour layer comprises a fiber fabric and a second aerogel reinforcement, and preferably, the second aerogel reinforcement is a phenolic aerogel; and / or

[0025] The gas barrier layer is one or more of silica gel, latex and fluororubber.

[0026] Compared with the prior art, the present invention has at least the following beneficial effects:

[0027] The deformable heat-insulating wave-absorbing material provided by the present invention is obtained by compounding a fiber matrix composed of silicon carbide fiber and oxide ceramic fiber with aerogel. The high thermal conductivity of silicon carbide is used to diffuse heat in a direction to avoid local high-temperature bulges in the heat-insulating material. The high-temperature resistance, high strength and wave-absorbing properties of silicon carbide are used to meet the stealth requirements of the heat-insulating material in a high-temperature aerobic environment. The oxide ceramic fiber is used to improve the heat-insulating performance and portable function of the heat-insulating material. The fibers in the deformable heat-insulating wave-absorbing material are formed into an integrated structure under the bonding action of the aerogel, and the shape is well maintained. Compared with other adhesives, aerogel can further reduce the thermal conductivity of the composite material and improve the heat-insulating effect of the composite material.

[0028] The deformable heat-insulating and wave-absorbing material structural unit with an origami structure provided by the present invention is controllable. Under high temperature and room temperature conditions, the deformation modes are various, large-scale deformation can be achieved, the deformation process is continuous and the shape can be restored, and the fatigue resistance is excellent. At the same time, it has wave-absorbing and stealth performance. Compared with the existing rigid insulation tiles and flexible insulation felts, it can better adapt to the multi-task aerodynamic shape transformation of high-speed variant aircraft and meet the aircraft's requirements for the stealth performance of insulation materials.

[0029] The deformable heat-insulating and wave-absorbing material provided by the present invention has a simple molding process and the parameters can be flexibly adjusted. The obtained heat-insulating and wave-absorbing material has the characteristics of flexibility, high temperature resistance, stealth, heat insulation, and large-scale deformation. It is a lightweight, efficient, multifunctional, and portable material. It can be used as a portable stealth heat-insulating filling material and can be used in various scenarios in the field of stealth thermal protection.

[0030] The skin provided by the present invention includes an anti-scour layer, a heat-insulating absorbing layer and an air-barrier layer, wherein the anti-scour layer includes a fiber fabric and a second aerogel reinforcement, and the aerogel tightly combines the fiber filaments, reducing the burr feeling of the fiber bundle, and the fiber bundle has higher strength, which can improve the anti-scour performance of the surface of the skin material. The heat-insulating absorbing layer is a deformable heat-insulating absorbing material with an origami structure, and the structural unit is adjustable. Under high temperature and room temperature conditions, the deformation mode is diverse, and large-scale deformation can be achieved. The deformation process is continuous and the shape can be restored. It has excellent fatigue resistance and has wave-absorbing stealth performance. It can better adapt to the multi-task aerodynamic shape transformation of high-speed variant aircraft and meet the aircraft's requirements for the stealth performance of heat-insulating materials. The air-barrier layer has excellent air tightness, which can ensure the air tightness of the skin material.

[0031] The skin provided by the present invention is a highly elastic, heat-resistant, deformable, multifunctional thermal protection material, which has the rigidity of load-bearing outside the plane and the flexibility of deforming inside the plane. It can achieve continuous, seamless, large-scale deformation under high and low temperature conditions, and has excellent heat insulation and wave absorption effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 It is a structural schematic diagram of a deformable heat-insulating and wave-absorbing material with a Miura origami structure provided by the present invention;

[0034] Figure 2 is a frequency-reflection loss curve of a deformable heat-insulating and wave-absorbing material having a Miura origami structure provided in Example 3 of the present invention;

[0035] Figure 3 It is a structural schematic diagram of a skin provided by the present invention;

[0036] Figure numerals: 11 - anti-scour layer; 12 - heat insulation and wave absorbing layer; 121 - silicon carbide fiber layer; 122 - oxide ceramic fiber layer; 13 - gas barrier layer. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] In a first aspect, the present invention provides a high temperature resistant flexible deformable heat insulating and wave absorbing material, such as Figure 1 As shown, the deformable heat-insulating and wave-absorbing material includes a fiber matrix with an origami structure and a first aerogel reinforcement.

[0039] The fiber matrix includes a silicon carbide fiber layer and an oxide ceramic fiber layer.

[0040] It should be noted that the fiber matrix includes at least one silicon carbide fiber layer and one oxide ceramic fiber layer, and the number of silicon carbide fiber layers and oxide ceramic fiber layers can be adjusted according to actual use requirements.

[0041] The deformable heat-insulating wave-absorbing material provided by the present invention is obtained by compounding a fiber matrix composed of silicon carbide fiber and oxide ceramic fiber with aerogel. The high thermal conductivity of silicon carbide is used to diffuse heat in a direction to avoid local high-temperature bulges in the heat-insulating material. The high-temperature resistance, high strength and wave-absorbing properties of silicon carbide are used to meet the stealth requirements of the heat-insulating material in a high-temperature aerobic environment. The oxide ceramic fiber is used to improve the heat-insulating performance and portable function of the heat-insulating material. The fibers in the deformable heat-insulating wave-absorbing material are formed into an integrated structure under the bonding action of the aerogel, and the shape is well maintained. Compared with other adhesives, aerogel can further reduce the thermal conductivity of the composite material and improve the heat-insulating effect of the composite material.

[0042] The deformable heat-insulating and wave-absorbing material structural unit with an origami structure provided by the present invention is controllable. Under high temperature and room temperature conditions, the deformation modes are various, large-scale deformation can be achieved, the deformation process is continuous and the shape can be restored, and the fatigue resistance is excellent. At the same time, it has wave-absorbing and stealth performance. Compared with the existing rigid insulation tiles and flexible insulation felts, it can better adapt to the multi-task aerodynamic shape transformation of high-speed variant aircraft and meet the aircraft's requirements for the stealth performance of insulation materials.

[0043] The deformable heat-insulating and wave-absorbing material provided by the present invention has a simple molding process and the parameters can be flexibly adjusted. The obtained heat-insulating and wave-absorbing material has the characteristics of flexibility, high temperature resistance, stealth, heat insulation, and large-scale deformation. It is a lightweight, efficient, multifunctional, and portable material. It can be used as a portable stealth heat-insulating filling material and can be used in various scenarios in the field of stealth thermal protection.

[0044] In order to obtain good aerodynamic and stealth performance at the same time, the present invention is based on the principle of combining shape stealth technology with material stealth technology. The prepared deformable thermal insulation material can be used as a sandwich structure, and its portable characteristics can be utilized to cooperate with the aircraft to change the shape and combine characteristics. The deformable thermal insulation material's own wave-absorbing properties can be used to improve the stealth performance, thereby solving the stealth development needs of radar and improving the aircraft's combat capability and intelligence level.

[0045] According to some preferred embodiments, the oxide ceramic fiber layer includes one or more of silica fiber, alumina fiber, and mullite fiber.

[0046] In some preferred embodiments of the present invention, the oxide ceramic fiber layer is one or more of oxide fibers and oxide fiber fabrics, preferably one or more of silica fibers, alumina fibers, mullite fibers, silica fiber fabrics, alumina fiber fabrics, and mullite fiber fabrics.

[0047] According to some preferred embodiments, the thickness of the silicon carbide fiber layer is 0.5-1 mm (for example, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm or 1 mm).

[0048] In some preferred embodiments of the present invention, the silicon carbide fiber layer is one or more of silicon carbide fiber and silicon carbide fiber fabric, preferably one or more of silicon carbide long fiber, silicon carbide 2.5D woven fabric, and silicon carbide fiber knitted fabric.

[0049] According to some preferred embodiments, the thickness of the oxide ceramic fiber layer is 1 to 10 mm (for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm or 10 mm).

[0050] According to some preferred embodiments, the first aerogel reinforcement is one or more of silica aerogel, alumina aerogel, aluminum-silicon aerogel, SiOC aerogel, and SiOCN aerogel; preferably, the first aerogel reinforcement accounts for 30 to 60% of the total mass of the deformable thermal insulation and absorbing material (for example, it can be 30%, 35%, 40%, 45%, 50%, 55% or 60%).

[0051] According to some preferred embodiments, the origami structure is at least one of a Z-shaped origami structure, a Flasher origami structure, and a Miura origami structure. The present invention selects a molding method according to the structure and deformation performance of the fiber matrix to be molded; under the same other conditions, the deformation performance (deformation amount): semi-manual folding molding> extrusion molding> press molding.

[0052] The deformable heat-insulating and wave-absorbing material with an origami structure of the present invention can realize continuous movement along a predetermined fold, has a large-size deformation capability (the in-plane variable area deformation is not less than 30%), and can recover its shape after being stretched and deformed, and the structure is not easily damaged. Among them, the Z-shaped origami structure can realize the height contraction of a large plane in the horizontal or vertical direction, so that the volume of the overall structure is greatly reduced. The deformable heat-insulating and wave-absorbing material with a Z-shaped origami structure can realize in-plane deformation in one-dimensional direction (the in-plane variable area deformation is not less than 30%). The Flasher origami structure has the remarkable feature of a large folding and unfolding ratio. The deformable heat-insulating and wave-absorbing material with the Flasher origami structure can realize a large in-plane deformation (the in-plane variable area deformation is not less than 30%) and out-of-plane deformation (the out-of-plane bulging deformation is not less than 20%), and has a three-dimensional deformation capability. The Miura origami structure can be folded simultaneously in two directions perpendicular to each other, and can bulge outward. The deformable heat-insulating and wave-absorbing material with the Miura origami structure can achieve in-plane x and y bidirectional deformation (in-plane variable area deformation is not less than 30%) and out-of-plane deformation (out-of-plane bulging deformation is not less than 20%), and has three-dimensional deformation capability.

[0053] The density of the deformable heat-insulating and wave-absorbing material with origami structure of the present invention is 0.2-0.6 g / cm 3 , thermal conductivity is no more than 0.05W / m·K, in-plane deformation is no less than 30%, and it has excellent deformation performance.

[0054] In a second aspect, the present invention provides a method for preparing the deformable heat-insulating and wave-absorbing material according to the first aspect, the preparation method comprising the following steps:

[0055] Pre-treating and molding the fibers to obtain a fiber matrix;

[0056] The fiber matrix is ​​immersed in a first aerogel precursor impregnation liquid, and subjected to heat treatment, solvent replacement, and drying to obtain the deformable heat-insulating and wave-absorbing material.

[0057] According to some preferred embodiments, pyrolysis is further included after the drying, and the pyrolysis temperature is 900-1200°C (for example, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C or 1200°C).

[0058] In the process of preparing the deformable heat-insulating and wave-absorbing material of the present invention, when the first aerogel is a silica aerogel, an alumina aerogel, or an aluminum-silicon aerogel, after the fiber matrix is ​​impregnated with the first aerogel precursor impregnation liquid, it is subjected to heat treatment, solvent replacement, and drying to obtain the deformable heat-insulating and wave-absorbing material. When the first aerogel is a SiOC aerogel or a SiOCN aerogel, after the fiber matrix is ​​impregnated with the first aerogel precursor impregnation liquid, it is subjected to heat treatment, solvent replacement, and drying, and then pyrolysis is required to obtain the deformable heat-insulating and wave-absorbing material. The pyrolysis of the present invention needs to be carried out under a protective atmosphere, and the protective gas is preferably argon or nitrogen.

[0059] According to some preferred embodiments, the first aerogel precursor impregnation liquid includes a first aerogel precursor, an organic solvent and a catalyst; preferably, the first aerogel precursor accounts for 20-50% of the total mass of the first aerogel precursor impregnation liquid (for example, it can be 20%, 22%, 25%, 26%, 28%, 30%, 32%, 35%, 36%, 38%, 40%, 42%, 45%, 48% or 50%). If the content of the first aerogel precursor is too large, it will lead to excessive aerogel filling in the composite material, resulting in accumulation of aerogel in the pores, increased solid-phase heat transfer, and increased thermal conductivity of the composite material. If the content of the first aerogel precursor is too small, the pores of the composite material will increase, resulting in excessive thermal conductivity of the composite material.

[0060] Preferably, the first aerogel precursor is at least one of a silicon source and an aluminum source; more preferably, the silicon source is one or more of water glass, tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trimethylmethoxysilane, hexamethyldisilazane, and aminopropyltriethoxysilane; more preferably, the aluminum source is one or more of aluminum sec-butoxide, aluminum isopropoxide, aluminum chloride hexahydrate, and aluminum nitrate nonahydrate;

[0061] Preferably, the organic solvent is an alcohol, preferably one or more of methanol, ethanol, isopropanol and n-propanol;

[0062] Preferably, the catalyst is an acid solution or an alkaline solution, and the acid solution is preferably one or more of hydrochloric acid, acetic acid and nitric acid; the alkaline solution is preferably one or more of ammonia water and sodium hydroxide solution; more preferably, the concentrations of the acid solution and the alkaline solution are independently 0.3 to 0.6 mol / L (for example, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L, 0.45 mol / L, 0.5 mol / L, 0.55 mol / L or 0.60 mol / L). If the catalyst concentration is high, the gelation speed is too fast, and the fiber matrix cannot be completely impregnated. The gelation time of the present invention is 1 min to 30 min, and the higher the concentration, the faster the gelation speed.

[0063] According to some preferred embodiments, the pretreatment includes laying, cutting, and impregnating the fibers; the fibers need to be pretreated before forming the fiber matrix, specifically: laying the fibers to a desired thickness, cutting them to a desired size, impregnating them, and then forming them through a mold. The thickness of the fiber laying and the cutting size can be selected according to actual needs.

[0064] According to some preferred embodiments, the molding includes at least one of pressing molding, extrusion molding, and semi-manual folding molding; the present invention selects the molding method according to the structure of the fiber matrix to be finally molded.

[0065] According to some preferred embodiments, after forming, the process further includes the steps of drying the fiber matrix and fixing the structure; the solvent in the fiber is removed by drying, and the formed fiber matrix is ​​placed in a container for structural fixation.

[0066] According to some preferred embodiments, the drying temperature is 80-100°C (for example, 80°C, 85°C, 90°C, 95°C or 100°C), and the drying time is 8-12h (for example, 8h, 9h, 10h, 11h or 12h).

[0067] According to some preferred embodiments, the immersion time is 5 to 15 minutes (for example, 5 minutes, 10 minutes or 15 minutes).

[0068] According to some preferred embodiments, the heat treatment temperature is 30-60°C (for example, 30°C, 32°C, 35°C, 38°C, 40°C, 42°C, 45°C, 48°C, 50°C, 55°C, 58°C or 60°C).

[0069] According to some preferred embodiments, the solvent used in the solvent replacement is ethanol or acetone.

[0070] According to some preferred embodiments, the drying method is at least one of normal pressure drying and supercritical drying.

[0071] The present invention provides a skin in a third aspect, such as Figure 3 The skin includes an anti-scour layer 11, a heat-insulating and wave-absorbing layer 12 and a gas-barrier layer 13 from the outside to the inside, and the heat-insulating and wave-absorbing layer is the deformable heat-insulating and wave-absorbing material described in the first aspect.

[0072] It should be noted that the deformable heat-insulating and wave-absorbing material includes at least one silicon carbide fiber layer 121 and one oxide ceramic fiber layer 122 , and the silicon carbide fiber layer 121 is located on the side close to the anti-scour layer 11 .

[0073] The drawings of the present invention are provided for illustration purposes only, and the proportions of the components in the drawings may not necessarily be consistent with the actual product. Figure 3 In the figure, the structural layers are peeled off from each other, which is to clearly show the positional relationship between the structural layers of the present invention. However, it should be understood that in the present invention, the structural layers are actually tightly fitted and / or partially fitted.

[0074] The skin provided by the present invention includes an anti-scour layer, a heat-insulating absorbing layer and an air-barrier layer, wherein the anti-scour layer includes a fiber fabric and a second aerogel reinforcement, and the aerogel tightly combines the fiber filaments, reducing the burr feeling of the fiber bundle, and the fiber bundle has higher strength, which can improve the anti-scour performance of the surface of the skin material. The heat-insulating absorbing layer is a deformable heat-insulating absorbing material with an origami structure, and the structural unit is adjustable. Under high temperature and room temperature conditions, the deformation mode is diverse, and large-scale deformation can be achieved. The deformation process is continuous and the shape can be restored. It has excellent fatigue resistance and has wave-absorbing stealth performance. It can better adapt to the multi-task aerodynamic shape transformation of high-speed variant aircraft and meet the aircraft's requirements for the stealth performance of heat-insulating materials. The air-barrier layer has excellent air tightness, which can ensure the air tightness of the skin material.

[0075] The skin provided by the present invention is a highly elastic, heat-resistant, deformable, multifunctional thermal protection material, which has the rigidity of load-bearing outside the plane and the flexibility of deforming inside the plane. It can achieve continuous, seamless, large-scale deformation under high and low temperature conditions, and has excellent heat insulation and wave absorption effects.

[0076] In addition, the preparation method of the skin provided by the present invention is simple, and can be combined with other materials, integrating multi-functions and uses, and has a wide range of applications.

[0077] According to some preferred embodiments, the anti-scour layer includes a fiber fabric and a second aerogel reinforcement; preferably, the second aerogel reinforcement is a phenolic aerogel.

[0078] According to some preferred embodiments, the gas barrier layer is one or more of silica gel, latex, and fluororubber.

[0079] In some preferred embodiments of the present invention, the method for preparing the anti-scour layer comprises: placing the fiber fabric in a second aerogel precursor impregnation solution, and performing curing and drying to obtain the anti-scour layer.

[0080] In some preferred embodiments of the present invention, the anti-scour layer, the heat-insulating and wave-absorbing layer and the gas-barrier layer are combined into an integrated structure by sewing with sutures.

[0081] In some preferred embodiments of the present invention, the suturing method adopts at least one of an "O-type" orientation and a "Z-type" orientation.

[0082] In some preferred embodiments of the present invention, the second aerogel precursor impregnation liquid comprises a second aerogel precursor, a solvent and a curing agent; preferably, the volume of the second aerogel precursor is 5 to 20% of the volume of the solvent (for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%); preferably, the second aerogel precursor is a phenolic resin.

[0083] In some preferred embodiments of the present invention, the curing temperature is 100-150° C. (for example, 100° C., 110° C., 120° C., 130° C., 140° C. or 150° C.).

[0084] In some preferred embodiments of the present invention, the fiber fabric is made of one or more of quartz fiber, glass fiber, alumina fiber, and mullite fiber;

[0085] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with embodiments.

[0086] The present invention does not specifically limit the sources of the reagents used in the examples and comparative examples, and the reagents can be directly purchased or synthesized.

[0087] The performance data testing method of the heat-insulating and wave-absorbing materials and skins prepared in the embodiments of the present invention and the comparative examples is as follows:

[0088] Thermal conductivity: The flat plate heat flow meter method is used, and the test standard refers to "Determination of steady-state thermal resistance and related properties of insulation materials - Heat flow meter method GB / T 10295-2008".

[0089] Deformation performance (in-plane deformation and out-of-plane deformation): tested using a universal testing machine; the thermal insulation material and skin prepared in the embodiments and comparative examples were stretched in the plane, and the structures of the thermal insulation material and the skin were recoverable, and the maximum deformation without destroying the structure was the in-plane deformation; the thermal insulation material and the skin prepared in the embodiments and comparative examples were bulged out-of-plane, and the structures of the thermal insulation material and the skin were recoverable, and the maximum deformation without destroying the structure was the out-of-plane deformation.

[0090] Example 1

[0091] A high-temperature resistant flexible deformable heat-insulating and wave-absorbing material comprises a fiber matrix with a Flasher origami structure and a first aerogel reinforcement; the fiber matrix comprises a silica fiber layer and a silicon carbide long fiber layer, the first aerogel reinforcement is a silica aerogel, and the silica aerogel accounts for 50% of the total mass of the deformable heat-insulating and wave-absorbing material.

[0092] A method for preparing a high temperature resistant flexible deformable heat insulating and wave absorbing material comprises the following steps:

[0093] (1) Preparation of sol: Tetramethoxysilane and methanol are mixed and stirred for 30 minutes to obtain a tetramethoxysilane solution, wherein tetramethoxysilane accounts for 30 wt.% of the tetramethoxysilane solution; ammonia water and distilled water are mixed and stirred to a concentration of 0.3 mol / L; the diluted ammonia solution is poured into the tetramethoxysilane solution and stirred for 2 minutes.

[0094] (2) Preparation of fiber matrix: Lay silica fibers with a thickness of 2 mm and cut them into a size of 150 mm × 200 mm. Then, lay long silicon carbide fibers on the silica fiber layer according to a rule with a thickness of 0.5 mm and a size of 150 mm × 200 mm. Then, use distilled water to wet the laid fibers. Then, press them through a mold to form a Flasher origami structure. After molding, fix them in an 80 mm × 80 mm polytetrafluoroethylene mold and put them in an oven for drying at a temperature of 100 ° C for 8 h to obtain a fiber matrix.

[0095] (3) Preparing a deformable heat-insulating and wave-absorbing material: impregnating the fiber matrix prepared in step (2) into the sol prepared in step (1), and vacuum impregnating for 5 minutes to allow the sol to completely impregnate the fiber matrix; heat-treating the fiber matrix impregnated with the sol at a constant temperature of 30° C. for 24 hours, then replacing the solvent with ethanol, soaking for 3 days, replacing the solvent every 12 hours, and finally supercritical drying to obtain a high-temperature resistant flexible deformable heat-insulating and wave-absorbing material.

[0096] The high temperature resistant flexible deformable heat insulating and wave absorbing material with Flasher origami structure prepared in this embodiment has a size of 80 mm×80 mm and a density of 0.4 g / cm 3 , the thermal conductivity is 0.032W / m·K, and it can achieve large in-plane deformation (deformation reaches 35%) and out-of-plane deformation (deformation reaches 20%). The shape can be restored after stretching, and the reflection loss is -13dB.

[0097] Example 2

[0098] A high-temperature resistant flexible deformable heat-insulating and wave-absorbing material includes a fiber matrix with a Z-shaped origami structure and a first aerogel reinforcement; the fiber matrix includes an alumina fiber layer and a silicon carbide 2.5D woven fabric, the first aerogel reinforcement is an alumina aerogel, and the alumina aerogel accounts for 40% of the total mass of the deformable heat-insulating and wave-absorbing material.

[0099] A method for preparing a high temperature resistant flexible deformable heat insulating and wave absorbing material comprises the following steps:

[0100] (1) preparing the sol: mixing ethanol and distilled water at 60° C. for 30 minutes, then adding aluminum sec-butoxide, and mixing and stirring for another 30 minutes; mixing concentrated nitric acid and distilled water for 10 minutes, then pouring into the aluminum sec-butoxide solution and stirring for 30 minutes, wherein the molar ratio of aluminum sec-butoxide: ethanol: distilled water: nitric acid is 1:7:0.65:0.02.

[0101] (2) Preparation of fiber matrix: alumina fibers are laid out in a regular pattern with a thickness of 3 mm. After being cut into a size of 100 mm × 100 mm, a silicon carbide 2.5D woven fabric with a size of 100 mm × 100 mm and a thickness of 0.8 mm is stacked on top of the alumina fiber layer, and then the fibers are impregnated with ethanol. The fibers are then extruded through a mold to form a Z-shaped origami structure. After molding, the structure is fixed in a 50 mm × 100 mm polytetrafluoroethylene mold and placed in an oven for drying at a temperature of 80 ° C for 12 h to obtain a fiber matrix.

[0102] (3) Preparing a deformable heat-insulating and wave-absorbing material: impregnating the fiber matrix prepared in step (2) into the sol prepared in step (1), vacuum impregnating for 10 minutes, allowing the sol to completely infiltrate the fiber matrix; and heat-treating the fiber matrix infiltrated with the sol at a constant temperature of 50° C. for 24 hours, then replacing the solvent with ethanol, soaking for 3 days, replacing the solvent every 12 hours, and finally supercritical drying to obtain a high-temperature resistant flexible deformable heat-insulating and wave-absorbing material.

[0103] The high temperature resistant flexible deformable heat insulating and wave absorbing material with a Z-shaped origami structure prepared in this embodiment has a size of 50 mm×100 mm and a density of 0.5 g / cm 3 , the thermal conductivity is 0.036W / m·K, a large in-plane deformation can be achieved (the deformation reaches 48%), and the shape can be restored after stretching, and the reflection loss is -16dB.

[0104] Example 3

[0105] A high-temperature resistant flexible deformable heat-insulating and wave-absorbing material comprises a fiber matrix with a Miura origami structure and a first aerogel reinforcement; the fiber matrix comprises a mullite fiber layer and a silicon carbide knitted fabric, and the first aerogel reinforcement is an aluminum-silicon aerogel, which accounts for 30% of the total mass of the deformable heat-insulating and wave-absorbing material.

[0106] A method for preparing a high temperature resistant flexible deformable heat insulating and wave absorbing material comprises the following steps:

[0107] (1) preparing sol: mixing ethanol and distilled water at 60° C. for 30 minutes, adding aluminum isopropoxide, and mixing for another 30 minutes, wherein the molar ratio of aluminum isopropoxide: ethanol: distilled water is 1:12:0.6; mixing tetraethoxysilane, distilled water, ethanol, and hydrochloric acid for 30 minutes, wherein the molar ratio of tetraethoxysilane: distilled water: ethanol: hydrochloric acid is 1:1:5:0.0018; then blending the aluminum isopropoxide solution and the tetraethoxysilane solution, and stirring for 30 minutes, wherein the molar ratio of aluminum: silicon is 3:1.

[0108] (2) Preparation of fiber matrix: Mullite fibers are laid with a thickness of 5 mm and cut into a size of 200 mm × 200 mm. Silicon carbide knitted fabric with a size of 200 mm × 200 mm and a thickness of 0.6 mm is laid on the mullite fiber layer, and then the laid fibers are impregnated with distilled water. The fibers are then extruded through a mold to form a Miura origami structure. After molding, the structure is fixed in a 100 mm × 100 mm polytetrafluoroethylene mold and placed in an oven for drying at a temperature of 100 ° C. The heat treatment is performed for 12 h to obtain a fiber matrix.

[0109] (3) Preparing a deformable heat-insulating and wave-absorbing material: impregnating the fiber matrix prepared in step (2) into the sol prepared in step (1), and vacuum impregnating for 10 minutes to allow the sol to completely impregnate the fiber matrix; heat-treating the fiber matrix impregnated with the sol at a constant temperature of 60° C. for 24 hours, then replacing the solvent with ethanol, soaking for 3 days, replacing the solvent every 12 hours, and finally supercritical drying to obtain a high-temperature resistant flexible deformable heat-insulating and wave-absorbing material.

[0110] The high temperature resistant flexible deformable heat insulating and wave absorbing material with Miura origami structure prepared in this embodiment has a size of 100 mm×100 mm and a density of 0.5 g / cm 3 , the thermal conductivity is 0.042W / m·K, and it can achieve large in-plane deformation (deformation reaches 40%) and out-of-plane deformation (deformation reaches 25%). The shape can be restored after stretching, and the reflection loss is -18dB.

[0111] Example 4

[0112] A high-temperature resistant flexible deformable heat-insulating and wave-absorbing material comprises a fiber matrix with a Miura origami structure and a first aerogel reinforcement; the fiber matrix comprises a mullite fiber layer and a silicon carbide long fiber layer, the first aerogel reinforcement is SiOC aerogel, and the SiOC aerogel accounts for 30% of the total mass of the deformable heat-insulating and wave-absorbing material.

[0113] A method for preparing a high temperature resistant flexible deformable heat insulating and wave absorbing material comprises the following steps:

[0114] (1) preparing a sol: stirring tetraethoxysilane, methyltrimethoxysilane, hexamethyldisilazane and dimethyldiethoxysilane at room temperature for 30 min; adding a mixture of hydrochloric acid and distilled water to the siloxane solution and continuing to stir for 30 min; then adding a mixture of ammonia water and distilled water to the siloxane solution and continuing to stir for 30 min to obtain a sol solution, wherein the molar ratio of tetraethoxysilane: methyltrimethoxysilane: hexamethyldisilazane: dimethyldiethoxysilane: hydrochloric acid: ammonia water is 1:0.5:0.65:0.3:0.017:0.035.

[0115] (2) Preparation of fiber matrix: Mullite fibers are layered with a thickness of 2 mm and cut into a size of 200 mm × 200 mm. Silicon carbide long fibers are then layered on the mullite fiber layer with a thickness of 0.5 mm and cut into a size of 200 mm × 200 mm. This layering process is repeated three times, i.e., from top to bottom: silicon carbide fiber layer-mullite fiber layer-silicon carbide fiber layer-mullite fiber layer-silicon carbide fiber layer-mullite fiber layer. The fibers are then impregnated with distilled water. The fibers are then semi-manually folded to form a Miura origami structure. After forming, the structure is fixed in a 100 mm × 100 mm polytetrafluoroethylene mold and dried in an oven at 100 °C for 12 h to obtain a fiber matrix.

[0116] (3) Preparing a deformable heat-insulating and wave-absorbing material: impregnating the fiber matrix prepared in step (2) into the sol solution prepared in step (1), and vacuum impregnating for 15 minutes to allow the sol to completely impregnate the fiber matrix; and subjecting the obtained sol-impregnated fiber matrix to a constant temperature heat treatment of 30°C for 24 hours, and then replacing the solvent with ethanol, and soaking for 3 days, replacing the solvent every 12 hours. After the solvent replacement is completed, drying is performed at normal pressure. After drying, the composite material is pyrolyzed at 1000°C for 2 hours in an argon atmosphere to obtain a high-temperature resistant, flexible, deformable heat-insulating and wave-absorbing material.

[0117] The high temperature resistant flexible deformable heat insulating and absorbing material with Miura origami structure prepared in this embodiment has a size of 100 mm×100 mm and a density of 0.6 g / cm 3 , the thermal conductivity is 0.048W / m·K, and it can achieve large in-plane deformation (deformation reaches 38%) and out-of-plane deformation (deformation reaches 23%). The shape can be restored after stretching, and the reflection loss is -30dB.

[0118] Comparative Example 1

[0119] It is basically the same as Example 1, with the only difference being that the fiber matrix does not have an origami structure, that is, the silica fibers are layered with a layer thickness of 2 mm, and after being cut into a size of 80 mm × 80 mm, the silicon carbide long fibers are regularly laid on the silica fiber layer with a layer thickness of 0.5 mm and a layer size of 80 mm × 80 mm, and then the layered fibers are impregnated with distilled water; then they are formed by flat pressing with a mold, and placed in an oven for drying at a temperature of 100°C for 8 hours to obtain a fiber matrix with a size of 80 mm × 80 mm.

[0120] Since the fiber matrix does not reserve deformation during molding, the thermal insulation and absorbing material does not have the ability to deform, and cannot achieve in-plane deformation and out-of-plane deformation, or the structure is damaged during deformation.

[0121] Comparative Example 2

[0122] It is basically the same as Example 2, with the only difference being that the fiber matrix does not have an origami structure, the alumina fibers are regularly layered with a layer thickness of 3 mm, and after being cut into a size of 50 mm × 100 mm, a silicon carbide 2.5D woven fabric with a size of 50 mm × 100 mm and a thickness of 0.8 mm is superimposed on the alumina fiber layer, and then the fibers are impregnated with ethanol; then they are formed by flat pressing with a mold, and placed in an oven for drying at a temperature of 80°C for 12 hours to obtain a fiber matrix with a size of 50 mm × 100 mm.

[0123] Since the fiber matrix does not reserve deformation during molding, the thermal insulation and absorbing material does not have the ability to deform, and cannot achieve in-plane deformation and out-of-plane deformation, or the structure is damaged during deformation.

[0124] Comparative Example 3

[0125] It is basically the same as Example 3, with the only difference being that the fiber matrix does not have an origami structure, that is, the mullite fibers are layered with a layer thickness of 5 mm, and after being cut into a size of 100 mm × 100 mm, a silicon carbide knitted fabric with a size of 100 mm × 100 mm and a thickness of 0.6 mm is laid on the mullite fiber layer, and then the layered fibers are impregnated with distilled water; then they are formed by flat pressing with a mold, and placed in an oven for drying at a temperature of 100°C and heat treated for 12 hours to obtain a fiber matrix with a size of 100 mm × 100 mm.

[0126] Since the fiber matrix does not reserve deformation during molding, the thermal insulation and absorbing material does not have the ability to deform, and cannot achieve in-plane deformation and out-of-plane deformation, or the structure is damaged during deformation.

[0127] Comparative Example 4

[0128] It is basically the same as Example 4, with the only difference being that the fiber matrix does not have an origami structure, that is, the mullite fibers are layered with a layer thickness of 2 mm and cut into a size of 100 mm × 100 mm, and then the silicon carbide long fibers are layered on the mullite fiber layer with a layer thickness of 0.5 mm and cut into a size of 100 mm × 100 mm; this layering is repeated 3 times, that is, from top to bottom: silicon carbide fiber layer-mullite fiber layer-silicon carbide fiber layer-mullite fiber layer-silicon carbide fiber layer-mullite fiber layer, and then the fibers are impregnated with distilled water; then they are formed by flat pressing with a mold and placed in an oven for drying at a temperature of 100°C for 12 hours to obtain a fiber matrix with a size of 100 mm × 100 mm.

[0129] Since the fiber matrix does not reserve deformation during molding, the thermal insulation and absorbing material does not have the ability to deform, and cannot achieve in-plane deformation and out-of-plane deformation, or the structure is damaged during deformation.

[0130] Comparative Example 5

[0131] It is basically the same as Example 4, with the only difference being that the fiber matrix is ​​composed of a mullite fiber knitted fabric without an origami structure and a silicon carbide fiber knitted fabric; that is, a silicon carbide knitted fabric with a size of 100mm×100mm and a thickness of 0.5mm is laid on a mullite fiber knitted fabric with a size of 100mm×100mm and a thickness of 2mm, and this layering is repeated 3 times, that is, from top to bottom: silicon carbide fiber knitted fabric-mullite fiber knitted fabric-silicon carbide fiber knitted fabric-mullite fiber knitted fabric-silicon carbide fiber knitted fabric-mullite fiber knitted fabric, and then the fibers are impregnated with distilled water; then they are formed by flat pressing with a mold, and placed in an oven for drying at a temperature of 100°C for 12h to obtain a fiber matrix with a size of 100mm×100mm.

[0132] Although knitted fabrics have a certain degree of deformation ability, they have a large pore structure. When used as an aerogel carrier, aerogel can only attach to the fiber bundles of the fabric. If the aerogel completely fills the pore structure, the fabric will no longer have the ability to deform, and the resulting thermal insulation and absorbing material will not have the ability to deform.

[0133] Example 5

[0134] A skin comprises, from outside to inside, an anti-scour layer, a heat-insulating wave-absorbing layer and a gas-barrier layer; the anti-scour layer uses quartz fiber fabric as a matrix and phenolic aerogel as a reinforcement; the heat-insulating wave-absorbing layer is a Flasher origami structure deformable heat-insulating wave-absorbing material prepared in Example 1; and the gas-barrier layer is a silica gel material.

[0135] A method for preparing a skin, comprising:

[0136] (1) Preparation of an anti-scour layer: Phenolic powder, ethanol, and a curing agent are mixed and stirred for 90 minutes to obtain a phenolic solution, wherein the phenolic powder accounts for 10 vol% of the ethanol and the curing agent is 15 wt% of the phenolic powder; a fabric (a fabric knitted from quartz fibers, with a size of 80 mm×80 mm) is placed in a polytetrafluoroethylene container, and the phenolic solution is poured into the container so that the fabric is completely immersed. After standing for 10 minutes, the fabric is moved to a reactor and sealed. The reactor is placed in a 100° C. oven for 24 hours. Finally, the fabric is dried at normal pressure to obtain an anti-scour layer.

[0137] (2) Preparation of heat-insulating and wave-absorbing layer: See the preparation method of the deformable heat-insulating and wave-absorbing material in Example 1, with the size of the layer being 80 mm×80 mm.

[0138] (3) Preparation of deformable heat-resistant skin: The anti-scour layer, the heat-insulating and wave-absorbing layer and the gas-barrier layer (the silicone material with a size of 80 mm × 80 mm and a thickness of 1.5 mm) are combined with high-temperature resistant sutures, and the suture method adopts a "Z-type" direction.

[0139] The three-layer structure skin provided in this embodiment can achieve an in-plane variable area deformation of up to 30%, and an out-of-plane bulging deformation of up to 16%. The skin can meet the use requirements under high temperature conditions of 800°C.

[0140] Example 6

[0141] A skin comprises, from outside to inside, an anti-scour layer, a heat-insulating wave-absorbing layer and a gas-barrier layer; the anti-scour layer uses glass fiber fabric as a matrix and phenolic aerogel as a reinforcement; the heat-insulating wave-absorbing layer is a Z-shaped origami structure deformable heat-insulating wave-absorbing material prepared in Example 2; and the gas-barrier layer is a latex material.

[0142] A method for preparing a skin, comprising:

[0143] (1) Preparation of an anti-scour layer: Phenolic powder, ethanol, and a curing agent are mixed and stirred for 90 minutes to obtain a phenolic solution, wherein the phenolic powder accounts for 5 vol% of the ethanol and the curing agent is 18 wt% of the phenolic powder; a fabric (a fabric knitted from glass fibers, with a size of 50 mm×100 mm) is placed in a polytetrafluoroethylene container, and the phenolic solution is poured into the container so that the fabric is completely immersed. After standing for 10 minutes, the fabric is moved to a reactor and sealed. The reactor is placed in a 150° C. oven for 24 hours. Finally, the fabric is dried at normal pressure to obtain an anti-scour layer.

[0144] (2) Preparation of heat-insulating and wave-absorbing layer: See the preparation method of the deformable heat-insulating and wave-absorbing material in Example 2, with a size of 50 mm×100 mm.

[0145] (3) Preparation of deformable heat-resistant skin: The anti-scour layer, the heat-insulating and wave-absorbing layer and the gas-barrier layer (latex material with a size of 50 mm × 100 mm and a thickness of 1.0 mm) are combined with high-temperature resistant sutures, and the suture method adopts an "O-type" direction.

[0146] The three-layer structure skin provided in this embodiment can achieve an in-plane variable area deformation of up to 40%, and the skin can meet the use requirements under high temperature conditions of 800°C.

[0147] Example 7

[0148] A skin comprises, from outside to inside, an anti-scour layer, a heat-insulating wave-absorbing layer and a gas-barrier layer; the anti-scour layer uses quartz fiber fabric as a matrix and phenolic aerogel as a reinforcement; the heat-insulating wave-absorbing layer is a Miura origami structured deformable heat-insulating wave-absorbing material prepared in Example 3; and the gas-barrier layer is a latex material.

[0149] A method for preparing a skin, comprising:

[0150] (1) Preparation of an anti-scour layer: Phenolic powder, ethanol, and a curing agent are mixed and stirred for 90 minutes to obtain a phenolic solution, wherein the phenolic powder accounts for 12 vol% of the ethanol and the curing agent is used for 13 wt% of the phenolic powder; a fabric (a fabric knitted from quartz fibers, with a size of 100 mm×100 mm) is placed in a polytetrafluoroethylene container, and the phenolic solution is poured into the container so that the fabric is completely immersed. After standing for 10 minutes, the fabric is moved to a reactor and sealed. The reactor is placed in a 150° C. oven for 24 hours. Finally, the fabric is dried at normal pressure to obtain an anti-scour layer.

[0151] (2) Preparation of heat-insulating and wave-absorbing layer: See the preparation method of the deformable heat-insulating and wave-absorbing material in Example 3, with a size of 100 mm×100 mm.

[0152] (3) Preparation of deformable heat-resistant skin: The anti-scour layer, the heat-insulating and wave-absorbing layer and the gas-barrier layer (latex material with a size of 100 mm × 100 mm and a thickness of 0.5 mm) are combined with high-temperature resistant sutures, and the suture method adopts an "O-type" direction.

[0153] The three-layer structure skin provided in this embodiment can achieve an in-plane variable area deformation of up to 30%, and an out-of-plane bulging deformation of up to 20%. The skin can meet the use requirements under high temperature conditions of 800°C.

[0154] Example 8

[0155] A skin comprises, from outside to inside, an anti-scour layer, a heat-insulating wave-absorbing layer and a gas-barrier layer; the anti-scour layer uses an aluminum oxide fiber fabric as a matrix and a phenolic aerogel as a reinforcement; the heat-insulating wave-absorbing layer is a Miura origami structured deformable heat-insulating wave-absorbing material prepared in Example 4; and the gas-barrier layer is a fluororubber material.

[0156] A method for preparing a skin, comprising:

[0157] (1) Preparation of an anti-scour layer: Phenolic powder, ethanol, and a curing agent are mixed and stirred for 90 minutes to obtain a phenolic solution, wherein the phenolic powder accounts for 18 vol% of the ethanol and the curing agent is used for 20 wt% of the phenolic powder; a fabric (a fabric knitted from alumina fibers, with a size of 100 mm×100 mm) is placed in a polytetrafluoroethylene container, and the phenolic solution is poured into the container so that the fabric is completely immersed. After standing for 10 minutes, the fabric is moved to a reactor and sealed. The reactor is placed in a 150° C. oven for 24 hours. Finally, the fabric is dried at normal pressure to obtain an anti-scour layer.

[0158] (2) Preparation of heat-insulating and wave-absorbing layer: See the preparation method of the deformable heat-insulating and wave-absorbing material in Example 4, with a size of 100 mm×100 mm.

[0159] (3) Preparation of deformable heat-resistant skin: The anti-scour layer, the heat-insulating and wave-absorbing layer and the gas-barrier layer (the fluororubber material with a size of 100 mm × 100 mm and a thickness of 0.8 mm) are combined with high-temperature resistant sutures, and the suture method adopts an "O-type" direction.

[0160] The three-layer structure skin provided in this embodiment can achieve an in-plane variable area deformation of up to 18%, and an out-of-plane bulging deformation of up to 17%. The skin can meet the use requirements under high temperature conditions of 800°C.

[0161] Comparative Example 6

[0162] It is basically the same as Example 5, except that the heat insulation and wave absorbing layer is the heat insulation and wave absorbing material prepared in Comparative Example 1.

[0163] Since the fiber matrix does not have a reserved deformation amount during molding, the thermal insulation and wave absorbing layer does not have the ability to deform, resulting in the final three-layer structural skin material also not having the ability to deform.

[0164] Comparative Example 7

[0165] It is basically the same as Example 6, except that the heat insulation and wave absorbing layer is the heat insulation and wave absorbing material prepared in Comparative Example 2.

[0166] Since the fiber matrix does not have a reserved deformation amount during molding, the thermal insulation and wave absorbing layer does not have the ability to deform, resulting in the final three-layer structural skin material also not having the ability to deform.

[0167] Comparative Example 8

[0168] It is basically the same as Example 7, except that the heat insulation and wave absorbing layer is the heat insulation and wave absorbing material prepared in Comparative Example 3.

[0169] Since the fiber matrix does not have a reserved deformation amount during molding, the thermal insulation and wave absorbing layer does not have the ability to deform, resulting in the final three-layer structural skin material also not having the ability to deform.

[0170] Comparative Example 9

[0171] It is basically the same as Example 8, except that the heat insulation and wave absorbing layer is the heat insulation and wave absorbing material prepared in Comparative Example 4.

[0172] Since the fiber matrix does not have a reserved deformation amount during molding, the thermal insulation and wave absorbing layer does not have the ability to deform, resulting in the final three-layer structural skin material also not having the ability to deform.

[0173] Comparative Example 10

[0174] It is basically the same as Example 8, except that the heat insulation and wave absorbing layer is the heat insulation and wave absorbing material prepared in Comparative Example 5.

[0175] The anti-scour layer and heat-insulating and wave-absorbing layer of the skin are both fabric materials with a porous structure, and only the surface of the fiber bundles in the fabric has an aerogel layer, which cannot meet the requirements of thermal insulation performance. In a high-temperature environment, the gas barrier layer may easily fail due to excessive temperature.

[0176] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high temperature resistant flexible deformable heat insulating and wave absorbing material, characterized in that: The deformable heat-insulating and wave-absorbing material comprises a fiber matrix having an origami structure and a first aerogel reinforcement; The fiber matrix includes a silicon carbide fiber layer and an oxide ceramic fiber layer. The silicon carbide fiber layer is laid on the oxide ceramic fiber layer, and the laid fibers are pretreated and formed to obtain a fiber matrix with an origami structure; the fiber matrix is ​​immersed in a first aerogel precursor impregnation liquid, and subjected to heat treatment, solvent replacement, and drying to obtain the deformable thermal insulation and absorbing material; the origami structure is at least one of a Z-type origami structure, a Flasher origami structure, and a Miura origami structure.

2. The deformable heat-insulating and wave-absorbing material according to claim 1, characterized in that: The oxide ceramic fiber layer includes one or more of silica fiber, alumina fiber, and mullite fiber; The thickness of the silicon carbide fiber layer is 0.5-1 mm; and / or The thickness of the oxide ceramic fiber layer is 1-10 mm.

3. The deformable heat-insulating and wave-absorbing material according to claim 1, characterized in that: The first aerogel reinforcement is one or more of silica aerogel, alumina aerogel, aluminum-silicon aerogel, SiOC aerogel, and SiOCN aerogel.

4. The deformable heat-insulating and wave-absorbing material according to claim 3, characterized in that: The first aerogel reinforcement accounts for 30-60% of the total mass of the deformable heat-insulating and wave-absorbing material.

5. A method for preparing the deformable heat-insulating and wave-absorbing material according to any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: The laid fibers are pretreated and formed to obtain a fiber matrix with an origami structure; The fiber matrix is ​​immersed in a first aerogel precursor impregnation liquid, and subjected to heat treatment, solvent replacement, and drying to obtain the deformable heat-insulating and wave-absorbing material.

6. The preparation method according to claim 5, characterized in that: After the drying, pyrolysis is further included, and the pyrolysis temperature is 900-1200°C.

7. The preparation method according to claim 5 or 6, characterized in that: The first aerogel precursor impregnation liquid includes a first aerogel precursor, an organic solvent and a catalyst.

8. The preparation method according to claim 7, characterized in that: The first aerogel precursor accounts for 20-50% of the total mass of the first aerogel precursor impregnation liquid; The first aerogel precursor is at least one of a silicon source and an aluminum source; The organic solvent is alcohol; The catalyst is an acid solution or an alkaline solution.

9. The preparation method according to claim 8, characterized in that: The silicon source is one or more of water glass, tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, trimethylmethoxysilane, hexamethyldisilazane, and aminopropyltriethoxysilane; the aluminum source is one or more of aluminum sec-butoxide, aluminum isopropoxide, aluminum chloride hexahydrate, and aluminum nitrate nonahydrate; The organic solvent is one or more of methanol, ethanol, isopropanol and n-propanol; The acid solution is one or more of hydrochloric acid, acetic acid and nitric acid; the alkali solution is one or more of ammonia water and sodium hydroxide solution.

10. The preparation method according to claim 8, characterized in that: The concentrations of the acid solution and the alkaline solution are independently 0.3-0.6 mol / L.

11. The preparation method according to claim 5 or 6, characterized in that: The forming includes at least one of press forming, extrusion forming, and semi-manual folding forming; The heat treatment temperature is 30-60°C; and / or The drying method is at least one of normal pressure drying and supercritical drying.

12. A skin, characterized in that: The skin comprises an anti-scour layer, a heat-insulating and wave-absorbing layer and a gas-barrier layer which are sequentially arranged from the outside to the inside, and the heat-insulating and wave-absorbing layer is the deformable heat-insulating and wave-absorbing material according to any one of claims 1 to 4.

13. The skin according to claim 12, characterized in that The anti-scour layer comprises a fiber fabric and a second aerogel reinforcement, and the fiber fabric is placed in a second aerogel precursor impregnation solution, and is cured and dried to obtain the anti-scour layer; The second aerogel reinforcement is phenolic aerogel; and / or The gas barrier layer is one or more of silica gel, latex and fluororubber.