A solid electrolyte and its preparation method, application and electrochemical device

By exchanging the metal cations of the molecular sieve as protons and calcining them with alkali metal salts, the problems of low conductivity and stability of the molecular sieve were solved, and a solid electrolyte with high conductivity was prepared, achieving independent use and improved stability.

CN118054092BActive Publication Date: 2024-11-26SHANGHAI JIAOTONG UNIV
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410177871.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-08
Publication Date
2024-11-26
Estimated Expiration
2044-02-08

AI Technical Summary

Technical Problem

The existing molecular sieves have low ionic conductivity and cannot be used as solid electrolyte alone, which has problems with stability and water absorption.

Method used

By exchanging the metal cations of the molecular sieve into protons, a halogenation reaction is carried out to reduce the concentration of oxygen negative ions, and calcining with the molten alkali metal salt, alkali metal cations and anions are introduced into the molecular sieve pores to improve the ion conductivity.

Benefits of technology

A solid electrolyte with high ionic conductivity can be prepared, which can be used alone, improving the stability and transportation convenience of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118054092B_ABST
    Figure CN118054092B_ABST
Patent Text Reader

Abstract

The present invention provides a solid electrolyte and its preparation method, application and electrochemical device. The preparation method comprises: performing ion exchange on molecular sieve-Na in an acidic solution so that the cations in the pores of molecular sieve-Na are exchanged for protons; after washing and drying, water molecules evaporate to form molecular sieve-H, and oxygen in the aluminum oxide tetrahedron of molecular sieve-H combines with protons to form OH; OH in molecular sieve-H is exchanged for halogen X1 (X1=F, Cl, Br, I) by halogenation reaction to obtain molecular sieve-X1; molecular sieve-X1 and melted AX2 are calcined to obtain a solid electrolyte; the pH of the acidic solution is 1.2<pH<2.1; AX2 includes alkali metal halides and / or alkali metal sulfides; the calcination temperature is 300-500°C. The solid electrolyte has a high ionic conductivity and can be used alone as a solid electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a solid electrolyte and a preparation method, application and electrochemical device thereof. Background Art

[0002] In recent years, new energy vehicles represented by electric vehicles have rapidly occupied the automobile market. As the core component of electric vehicles, the performance of power batteries has a huge impact on the actual performance of electric vehicles. The chemical system of commercial power batteries is lithium-ion batteries. Compared with traditional lithium-ion batteries using electrolytes, all-solid-state lithium batteries use solid electrolytes instead of electrolytes and diaphragms, making the batteries thinner and smaller in size, thereby improving the energy density of the batteries and improving the safety performance of the batteries.

[0003] Solid-state batteries are composed of a positive electrode, a solid electrolyte, and a negative electrode. In recent years, molecular sieves have also been gradually used as solid electrolytes in battery systems. However, due to the low ionic conductivity of molecular sieves, it is usually difficult to use them directly as solid electrolytes, and they are often used in combination with polymer electrolytes or ionic liquids.

[0004] For example, Chinese patent document CN116666737A discloses a composite solid electrolyte, a lithium battery and a preparation method, wherein a molecular sieve is placed in a lithium salt solution for ion exchange to obtain a modified molecular sieve; a polymer, a lithium salt, the modified molecular sieve and a solvent are then mixed to obtain a composite polymer electrolyte; the composite polymer electrolyte is coated on a porous base membrane to obtain a composite solid electrolyte, thereby solving the problems of poor mechanical strength and low lithium ion conductivity of existing lithium batteries.

[0005] Chinese patent document CN111755734A discloses a molecular sieve-loaded sodium ion solid electrolyte and its preparation method and application. The solid electrolyte is prepared by using molecular sieve, ionic liquid and sodium salt as raw materials, thereby improving the ionic conductivity of the solid electrolyte.

[0006] The above two patent documents prepare solid electrolytes by combining molecular sieves with polymer electrolytes or ionic liquids. Such composite solid electrolytes are unstable in the air, easily absorb water, and are not conducive to transportation and storage.

[0007] Therefore, developing a molecular sieve-type solid electrolyte that not only has high ion conductivity but can also be used alone is a problem to be solved by those skilled in the art. Summary of the invention

[0008] The technical problem solved by the present invention is to overcome the defects of the prior art that the molecular sieve has low ion conductivity and cannot be used alone as a solid electrolyte, and to provide a solid electrolyte and its preparation method, application and electrochemical device. The solid electrolyte prepared by the present invention has high ion conductivity and can be used alone as a solid electrolyte.

[0009] Molecular sieves usually have the problem of low ion conductivity when used as solid electrolytes. The prior art generally uses molecular sieves in combination with polymer electrolytes or ionic liquids or introduces cations into molecular sieves to improve the ion conductivity of molecular sieves. The oxygen anions in the molecular sieves are easy to combine with the metal cations in the molecular sieves, thereby hindering the migration of cations and resulting in low ion conductivity. The present invention exchanges the metal cations of the molecular sieve for protons first, and after drying, the water molecules in the molecular sieve evaporate, so that the oxygen in the aluminum-oxygen tetrahedron of the molecular sieve combines with the protons to form OH; the OH in the molecular sieve is exchanged for halogens through a halogenation reaction, thereby reducing the concentration of oxygen anions in the molecular sieve and facilitating the migration of metal cations; in addition, in order to further increase the migration speed of metal cations, the molecular sieve obtained after the halogenation reaction is calcined with a molten alkali metal salt, so that the cations and anions in the alkali metal salt are introduced into the molecular sieve, and the anions in the alkali metal salt are arranged at the edge of the molecular sieve pores, so that the alkali metal cations can better shuttle freely in the pores, further increasing the migration rate of the alkali metal cations in the pores, thereby increasing the ionic conductivity of the solid electrolyte.

[0010] The present invention solves the above technical problems through the following technical solutions:

[0011] The present invention provides a method for preparing a solid electrolyte, which comprises the following steps: subjecting molecular sieve-Na to ion exchange in an acidic solution, so that cations in the pores of the molecular sieve-Na are exchanged for protons; after washing and drying, water molecules are evaporated to form molecular sieve-H, and oxygen in the aluminum oxide tetrahedron of the molecular sieve-H is combined with protons to form OH; OH in the molecular sieve-H is exchanged for halogen X1 (X1=F, Cl, Br, I) through a halogenation reaction to obtain molecular sieve-X1; and then calcining the molecular sieve-X1 and melted AX2, so that cations and anions in the AX2 can enter the pores of the molecular sieve-X1, so as to obtain the solid electrolyte AX2@molecular sieve-X1;

[0012] Wherein, the pH of the acidic solution is 1.2<pH<2.1; the AX2 comprises alkali metal halide and / or alkali metal sulfide; and the calcination temperature is 300-500°C.

[0013] In the present invention, the preparation method preferably comprises the following steps: subjecting molecular sieve-Na to ion exchange, washing and drying in an acidic solution to form molecular sieve-H; subjecting the molecular sieve-H to a halogenation reaction to obtain molecular sieve-X1; and calcining the molecular sieve-X1 and the melted AX2 to obtain the solid electrolyte AX2@molecular sieve-X1;

[0014] Wherein, the pH of the acidic solution is 1.2<pH<2.1; the AX2 comprises alkali metal halide and / or alkali metal sulfide; and the calcination temperature is 300-500°C.

[0015] In the present invention, during the ion exchange process in the acidic solution, the pH in the acidic solution has an important influence on the structure of the molecular sieve and the degree to which the cations in the molecular sieve pores are exchanged for protons. When the pH of the acid used is 1.2<pH<2.2, the higher the degree to which the cations in the molecular sieve pores are exchanged for protons, the more conducive it is to the subsequent entry of alkali metal salts.

[0016] In the present invention, during the halogenation reaction, compared with negative divalent oxygen, negative monovalent halogen ions generally have a lower ion potential (Φ=Z / r), and their binding force with alkali metal ions is weaker, which helps the rapid transport of alkali metal ions between pores.

[0017] In the present invention, the pore size of the molecular sieve-Na may be 0.5-100 nm.

[0018] In the present invention, the type of the molecular sieve-Na may be one or more of X-type, A-type, Y-type and ZSM-5-type, for example, X-type.

[0019] In the present invention, the molecular sieve-Na refers to a molecular sieve whose cation is Na ion.

[0020] In a specific embodiment, the type of the molecular sieve-Na is NaY type molecular sieve.

[0021] In the present invention, the Na in the molecular sieve-Na 2 The mass fraction of O can be 8%-15%, for example 12.5%. The mass fraction refers to Na 2 The mass of O is a percentage of the mass of the molecular sieve.

[0022] In the present invention, the silicon-aluminum ratio in the molecular sieve-Na can be 0.9-5. The silicon-aluminum ratio refers to SiO 2 / Al 2 O 3 molar ratio.

[0023] In the present invention, the pH of the acidic solution is preferably 1.8<pH<2.1, such as 2.0.

[0024] In the present invention, the acidic solution may include one or more of acetic acid, hydrochloric acid, benzoic acid, formic acid and salicylic acid, such as acetic acid.

[0025] In the present invention, the concentration of the acidic solution may be 1.5-4 mol / L, such as 2 mol / L or 3 mol / L.

[0026] In a specific embodiment, the acidic solution is 2 mol / L acetic acid.

[0027] In the present invention, the ratio of the mass of the molecular sieve-Na to the volume of the acidic solution may be 1:(40-80) g / mL, for example 1:50 g / mL.

[0028] In the present invention, the ion exchange is generally carried out at room temperature.

[0029] In the present invention, the ion exchange time may be 8-20 hours, for example 12 hours.

[0030] In the present invention, the ion exchange is preferably carried out under stirring. The stirring speed may be 200-800 rpm, for example 400 rpm.

[0031] In the present invention, the washing is generally performed with deionized water. The washing method may be suction filtration. The number of times of washing is generally more than three times.

[0032] In the present invention, the drying temperature may be 40-80° C., such as 60° C. The drying time may be 2-8 hours, such as 3 hours. The drying is generally performed in an oven.

[0033] In the present invention, during the halogenation reaction, the substance containing the halogen X1 may be a halogen element or an ammonium salt. The halogen element may be, for example, liquid bromine, chlorine gas or iodine element. When the halogen X1 is F, the ammonium salt may be ammonium fluoride or ammonium hydrogen fluoride.

[0034] In the present invention, the method of the halogenation reaction can be flexibly selected according to the form of the substance containing the halogen X1. For example, when the substance containing the halogen X1 is a halogen gas element, the molecular sieve-H and the halogen gas element can be subjected to chemical vapor deposition; when the substance containing the halogen X1 is a halogen liquid element, a halogen solid element or an ammonium salt, the molecular sieve-H and the substance containing the halogen X1 can be subjected to a solvothermal reaction.

[0035] The solvent thermal reaction is generally carried out in a reactor. During the solvent thermal process, the solvent selected may be deionized water and / or an alcohol solvent. The alcohol solvent may be ethanol. The temperature of the solvent thermal reaction may be 110-150° C., for example, 130° C. The time of the solvent thermal reaction may be 8-16 hours, for example, 12 hours.

[0036] In a specific embodiment, the halogenation reaction comprises the following steps: reacting a mixture containing the molecular sieve-H, liquid bromine and ethanol in a reactor at a temperature of 130° C. for 12 hours. The ratio of the mass of the molecular sieve-Na to the volume of the liquid bromine may be (1.2-1.6) mg / μL, such as 1.43 mg / μL. The ratio of the volume of the liquid bromine to the ethanol may be 0.001-0.2, such as 0.007.

[0037] In the present invention, the cation of AX2 preferably includes Li ions and / or K ions.

[0038] In the present invention, the anion of AX2 includes one or more of Cl ions, Br ions, S ions and Se ions.

[0039] In the present invention, the alkali metal halide may be an alkali metal chloride or an alkali metal bromide.

[0040] In the present invention, the alkali metal sulfide may be an alkali metal sulfide or an alkali metal selenide.

[0041] In the present invention, the AX2 may be a mixed salt of lithium chloride and potassium chloride, a mixed salt of lithium bromide and potassium bromide, or a mixed salt of lithium chloride and lithium nitrate, preferably a mixed salt of lithium chloride and potassium chloride.

[0042] In a specific embodiment, the AX2 is a mixed salt of lithium chloride and potassium chloride.

[0043] When the AX2 is a mixed salt of lithium chloride and potassium chloride, the molar ratio of the lithium chloride to the potassium chloride may be 1:(0.5-1.5), preferably 1:(0.8-1.2), for example 1:0.5, 1:1 or 1:1.5.

[0044] In a specific embodiment, the AX2 is a mixed salt of lithium bromide and potassium bromide.

[0045] When the AX2 is a mixed salt of lithium bromide and potassium bromide, the molar ratio of the lithium bromide to the potassium bromide may be 1:(0.5-1.5), for example, 1:1.

[0046] In a specific embodiment, the AX2 is a mixed salt of lithium chloride and lithium nitrate.

[0047] When the AX2 is a mixed salt of lithium chloride and lithium nitrate, the molar ratio of the lithium chloride to the lithium nitrate may be 1:(0.5-1.5), for example, 1:1.

[0048] In the present invention, the amount of the substance of AX2 is equal to the amount of Na in the molecular sieve. 2 The substance amount ratio of O is preferably (5-15):1, such as 4:1, 8:1, 9:1, 10:1 or 12:1.

[0049] In the present invention, the method for preparing the melted AX2 may include the following steps: melting AX2 with a high temperature gun, or heating and melting AX2 in a muffle furnace or a tube furnace.

[0050] In the present invention, the calcination is generally carried out in an air atmosphere. The calcination equipment is generally a muffle furnace.

[0051] In the present invention, the calcination temperature may be 350-500°C, such as 380°C, 400°C or 450°C.

[0052] In the present invention, the calcination time may be 8-20 hours, such as 10 hours or 15 hours.

[0053] In the present invention, the rate of heating to the calcination temperature may be 0.5-10°C / min, preferably 1-5°C / min, for example 3°C / min.

[0054] In the present invention, the calcination is preferably followed by washing and drying.

[0055] The washing is generally performed with deionized water and the number of washings is generally more than three times.

[0056] The drying temperature may be 40-80° C., such as 60° C. The drying time may be 2-8 hours, such as 3 hours. The drying is generally carried out in an oven.

[0057] The present invention also provides a solid electrolyte prepared by the above-mentioned method for preparing the solid electrolyte.

[0058] In the present invention, the cations in the solid electrolyte preferably include Li ions and / or K ions.

[0059] In the present invention, the anions in the solid electrolyte include one or more of Cl ions, Br ions, S ions and Se ions.

[0060] The present invention also provides a solid electrolyte, which is a molecular sieve type solid electrolyte, wherein the anions in the solid electrolyte include one or more of Cl ions, Br ions, S ions and Se ions.

[0061] In the present invention, the ionic conductivity of the solid electrolyte can be 1*10 -7 ~5*10 -3 S cm -1 , for example 9.95*10 -6 S cm -1 , 1.2*10 -5 S cm -1 , 2.15*10 -5 S cm -1 , 2.27*10 -5 S cm -1 ,3.33*10 -5 S cm -1 4.29*10 -5 S cm -1 , or 4.77*10 -5 S cm -1 、.

[0062] The present invention also provides a use of the solid electrolyte as described above in preparing a battery.

[0063] In the present invention, different types of cations in the solid electrolyte correspond to different types of batteries. For example, when the cations in the solid electrolyte are lithium ions, or lithium ions and potassium ions, it can be used as a lithium battery.

[0064] The present invention also provides an electrochemical device, which comprises the solid electrolyte as described above.

[0065] In the present invention, the electrochemical device is a battery, such as a lithium-ion battery.

[0066] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0067] The reagents and raw materials used in the present invention are commercially available.

[0068] The positive and progressive effects of the present invention are:

[0069] The solid electrolyte prepared by the present invention has high ion conductivity and can be used alone as a solid electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 This is the SEM image of the solid electrolyte prepared in Example 1. DETAILED DESCRIPTION

[0071] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0072] The NaY molecular sieve used in the following examples and comparative examples was purchased from Nanhua NKC, model NKY-7.

[0073] Example 1

[0074] At room temperature, 1g NaY molecular sieve (Na 2 O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0075] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0076] The LiCl-KCl salt melted by a high temperature gun and the molecular sieve-X1 were mixed (the molar ratio of LiCl and KCl was 1:1, and the sum of the molar ratio of LiCl and KCl was equal to the Na in the NaY molecular sieve). 2 The molar ratio of O is 8:1), and the solid electrolyte AX2@molecular sieve-X1 is obtained by calcining in a muffle furnace at a temperature of 380°C and a time of 10 hours. The temperature is raised to the calcination temperature at a rate of 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain a solid electrolyte AX2@molecular sieve-X1.

[0077] Example 2

[0078] At room temperature, 1g NaY molecular sieve (Na 2 O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0079] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0080] The LiCl-LiNO melted by high temperature gun 3 After mixing salt and molecular sieve-X1 (LiCl and LiNO 3 The molar ratio of LiCl and LiNO is 1:1. 3 The sum of the amount of substance of NaY molecular sieve 2 The molar ratio of O is 8:1), and the solid electrolyte AX2@molecular sieve-X1 is obtained by calcining in a muffle furnace at a temperature of 380°C and a time of 10 hours. The temperature is raised to the calcination temperature at a rate of 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain a solid electrolyte AX2@molecular sieve-X1.

[0081] Example 3

[0082] At room temperature, 1g NaY molecular sieve (Na 2 O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0083] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0084] The LiCl-KCl salt melted by a high temperature gun and the molecular sieve-X1 were mixed (the molar ratio of LiCl and KCl was 1:0.5, and the sum of the molar ratio of LiCl and KCl was equal to the Na in the NaY molecular sieve). 2 The molar ratio of O is 8:1), and the solid electrolyte AX2@molecular sieve-X1 is obtained by calcining in a muffle furnace at a temperature of 380°C and a time of 10 hours. The temperature is raised to the calcination temperature at a rate of 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain a solid electrolyte AX2@molecular sieve-X1.

[0085] Example 4

[0086] At room temperature, 1g NaY molecular sieve (Na 2 O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0087] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0088] The LiCl-KCl salt melted by a high temperature gun and the molecular sieve-X1 were mixed (the molar ratio of LiCl and KCl was 1:1.5, and the sum of the molar ratio of LiCl and KCl was equal to the Na in the NaY molecular sieve). 2 The molar ratio of O is 8:1), and the solid electrolyte AX2@molecular sieve-X1 is obtained by calcining in a muffle furnace at a temperature of 380°C and a time of 10 hours. The temperature is raised to the calcination temperature at a rate of 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain a solid electrolyte AX2@molecular sieve-X1.

[0089] Example 5

[0090] At room temperature, 1g NaY molecular sieve (Na 2 O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0091] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0092] After the LiBr-KBr salt melted by a high temperature gun and the molecular sieve-X1 were mixed (the molar ratio of LiBr to KBr was 1:1, and the sum of the molar ratio of LiBr and KBr was equal to the Na in the NaY molecular sieve), 2 The molar ratio of O is 8:1), and the solid electrolyte AX2@molecular sieve-X1 is obtained by calcining in a muffle furnace at a temperature of 380°C and a time of 10 hours. The temperature is raised to the calcination temperature at a rate of 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain a solid electrolyte AX2@molecular sieve-X1.

[0093] Example 6

[0094] At room temperature, 1g NaY molecular sieve (Na 2O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0095] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0096] The LiCl-KCl salt melted by a high temperature gun and the molecular sieve-X1 were mixed (the molar ratio of LiCl and KCl was 1:1, and the sum of the molar ratio of LiCl and KCl was equal to the Na in the NaY molecular sieve). 2 The molar ratio of O is 4:1), and the solid electrolyte AX2@molecular sieve-X1 is obtained by calcining in a muffle furnace at a temperature of 380°C and a time of 10 hours. The temperature is raised to the calcination temperature at a rate of 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain the solid electrolyte AX2@molecular sieve-X1.

[0097] Example 7

[0098] At room temperature, 1g NaY molecular sieve (Na 2 O mass fraction of 12.5%) was added into 50mL 2MHAc aqueous solution (pH of 2), stirred at 400rpm for 12h, the stirred solution was filtered and washed three times with deionized water, and then dried in an oven at 60℃ for 3h to obtain molecular sieve-H;

[0099] Halogenation reaction of molecular sieve-H: 700 μL of liquid bromine was dissolved in 100 mL of ethanol, molecular sieve-H was added, and solvent thermal reaction was carried out (carried out in a reactor at 130° C. for 12 h), followed by suction filtration, ethanol washing, and drying to obtain molecular sieve-X1;

[0100] The LiCl-KCl salt melted by a high temperature gun and the molecular sieve-X1 were mixed (the molar ratio of LiCl and KCl was 1:1, and the sum of the molar ratio of LiCl and KCl was equal to the Na in the NaY molecular sieve). 2 The molar ratio of O is 10:1), and the calcination is carried out in a muffle furnace at a temperature of 380°C and a calcination time of 10 hours. The rate of heating to the calcination temperature is 3°C / min. The calcined product is washed three times with an appropriate amount of deionized water and dried at 60°C for 3 hours to obtain a solid electrolyte AX2@molecular sieve-X1.

[0101] Comparative Example 1

[0102] Compared with Example 1, except that the 2M HAc aqueous solution was replaced by a 1M HCl aqueous solution (pH 0), the other operations and conditions were the same as those in Example 1.

[0103] Comparative Example 2

[0104] Compared with Example 1, except that the 2M HAc aqueous solution was replaced by a 0.1M HCl aqueous solution (pH 1), the other operations and conditions were the same as those in Example 1.

[0105] Comparative Example 3

[0106] Compared with Example 1, except that the 2M HAc aqueous solution was replaced by a 1M HAc aqueous solution (pH 2.2), the other operations and conditions were the same as those in Example 1.

[0107] Comparative Example 4

[0108] Compared with Example 1, except that the 2M HAc aqueous solution was replaced by a 0.1M HAc aqueous solution (pH 2.8), the other operations and conditions were the same as those in Example 1.

[0109] Effect Example

[0110] 1. Morphology characterization

[0111] Figure 1 This is the SEM image of the solid electrolyte prepared in Example 1.

[0112] 2. Ionic conductivity test

[0113] At room temperature 25°C, 300 mg of the solid electrolyte prepared in Examples 1-7 and Comparative Examples 1-4 was placed in a mold and formed into a thin sheet with a radius of 5 mm and a thickness of 3 mm at a pressure of 300 MPa. Both ends of the mold were connected to Autolab for electrochemical impedance testing. The test results are shown in Table 1.

[0114] Table 1

[0115] sample <![CDATA[Ionic conductivity (S·cm -1 )]]> Example 1 <![CDATA[4.77*10 -5 ]]> Example 2 <![CDATA[1.20*10 -5 ]]> Example 3 <![CDATA[2.15*10 -5 ]]> Example 4 <![CDATA[2.27*10 -5 ]]> Example 5 <![CDATA[9.95*10 -6 ]]> Example 6 <![CDATA[3.33*10 -5 ]]> Example 7 <![CDATA[4.29*10 -5 <!-- 7 -->]]> Comparative Example 1 <![CDATA[1.73*10 -8 ]]> Comparative Example 2 <![CDATA[5.35*10 -7 ]]> Comparative Example 3 <![CDATA[9.14*10 -6 ]]> Comparative Example 4 <![CDATA[6.61*10 -6 ]]>

[0116] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.

Claims

1. A method for preparing a solid electrolyte, characterized in that: The following steps are involved: The molecular sieve-Na is subjected to ion exchange in an acidic solution, so that the cations in the pores of the molecular sieve-Na are exchanged for protons; after washing and drying, the water molecules evaporate to form a molecular sieve-H, and the oxygen in the aluminum oxide tetrahedron of the molecular sieve-H combines with the protons to form OH; the OH in the molecular sieve-H is exchanged for a halogen X1 through a halogenation reaction, where X1=F, Cl, Br, I, to obtain a molecular sieve-X1; the molecular sieve-X1 and the melted AX2 are then calcined, so that the cations and anions in the AX2 can enter the pores of the molecular sieve-X1, thereby obtaining the solid electrolyte AX2@molecular sieve-X1; Wherein, the pH of the acidic solution is 1.2<pH<2.1; the AX2 includes alkali metal halide and / or alkali metal sulfide; the calcination temperature is 300-500℃; the halogenation reaction method is: when the substance containing the halogen X1 is a halogen gas element, the molecular sieve-H and the halogen gas element are subjected to chemical vapor deposition; when the substance containing the halogen X1 is a halogen liquid element, a halogen solid element or an ammonium salt, the molecular sieve-H and the substance containing the halogen X1 are subjected to a solvothermal reaction.

2. The method for preparing a solid electrolyte according to claim 1, characterized in that: The pore size of the molecular sieve-Na is 0.5-100 nm; And / or, the type of the molecular sieve-Na is one or more of X-type, A-type, Y-type and ZSM-5 type.

3. The method for preparing a solid electrolyte according to claim 2, characterized in that: The type of the molecular sieve-Na is NaY type molecular sieve.

4. The method for preparing a solid electrolyte according to claim 1 or 2, characterized in that: The pH of the acidic solution is 1.8<pH<2.1; and / or, the acidic solution comprises one or more of acetic acid, hydrochloric acid, benzoic acid, formic acid and salicylic acid; And / or, the concentration of the acidic solution is 1.5-4 mol / L.

5. The method for preparing a solid electrolyte according to claim 4, characterized in that: The pH of the acidic solution is 2.0; And / or, the acidic solution is acetic acid; And / or, the concentration of the acidic solution is 2 mol / L or 3 mol / L.

6. The method for preparing a solid electrolyte according to claim 1 or 2, characterized in that: The ratio of the mass of the molecular sieve-Na to the volume of the acidic solution is 1: (40-80) g / mL; And / or, the ion exchange time is 8-20h; And / or, the drying temperature is 40-80°C; And / or, the drying time is 2-8 hours.

7. The method for preparing a solid electrolyte according to claim 6, characterized in that: The ratio of the mass of the molecular sieve-Na to the volume of the acidic solution is 1:50 g / mL; And / or, the ion exchange time is 12h; And / or, the drying temperature is 60°C; And / or, the drying time is 3 hours.

8. The method for preparing a solid electrolyte according to claim 1 or 2, characterized in that: The cations of AX2 include Li ions and / or K ions; and / or, the anion of AX2 includes one or more of Cl ions, Br ions, S ions and Se ions; And / or, AX2 is a mixed salt of lithium chloride and potassium chloride, a mixed salt of lithium bromide and potassium bromide, or a mixed salt of lithium chloride and lithium nitrate; And / or, the ratio of the amount of AX2 to the amount of Na2O in the molecular sieve is (3-15):

1.

9. The method for preparing a solid electrolyte according to claim 8, characterized in that: The AX2 is a mixed salt of lithium chloride and potassium chloride.

10. The method for preparing a solid electrolyte according to claim 8, characterized in that: When the AX2 is a mixed salt of lithium chloride and potassium chloride, the molar ratio of the lithium chloride to the potassium chloride is 1:(0.5-1.5).

11. The method for preparing a solid electrolyte according to claim 10, characterized in that: When the AX2 is a mixed salt of lithium chloride and potassium chloride, the molar ratio of the lithium chloride to the potassium chloride is 1:(0.8-1.2).

12. The method for preparing a solid electrolyte according to claim 10, characterized in that: When the AX2 is a mixed salt of lithium chloride and potassium chloride, the molar ratio of the lithium chloride to the potassium chloride is 1:0.5, 1:1 or 1:1.

5.

13. The method for preparing a solid electrolyte according to claim 8, characterized in that: When the AX2 is a mixed salt of lithium bromide and potassium bromide, the molar ratio of the lithium bromide to the potassium bromide is 1:(0.5-1.5).

14. The method for preparing a solid electrolyte according to claim 13, characterized in that: When the AX2 is a mixed salt of lithium bromide and potassium bromide, the molar ratio of the lithium bromide to the potassium bromide is 1:

1.

15. The method for preparing a solid electrolyte according to claim 8, characterized in that: When the AX2 is a mixed salt of lithium chloride and lithium nitrate, the molar ratio of the lithium chloride to the lithium nitrate is 1:(0.5-1.5).

16. The method for preparing a solid electrolyte according to claim 15, characterized in that: When the AX2 is a mixed salt of lithium chloride and lithium nitrate, the molar ratio of the lithium chloride to the lithium nitrate is 1:

1.

17. The method for preparing a solid electrolyte according to claim 8, characterized in that: The ratio of the amount of AX2 to the amount of Na2O in the molecular sieve is 4:1, 8:1, 9:1, 10:1 or 12:

1.

18. The method for preparing a solid electrolyte according to claim 1 or 2, characterized in that: During the halogenation reaction, the substance containing the halogen X1 is a halogen element or an ammonium salt; and / or, the temperature of the solvent thermal reaction is 110-150° C.; And / or, the solvent thermal reaction time is 8-16h; And / or, the calcination temperature is 350-500°C; And / or, the calcination time is 8-20h.

19. The method for preparing a solid electrolyte according to claim 18, characterized in that: The halogen element is liquid bromine, chlorine gas or iodine element.

20. The method for preparing a solid electrolyte according to claim 18, characterized in that: The temperature of the solvothermal reaction is 130°C; And / or, the solvent thermal reaction time is 12h; and / or, the calcination temperature is 380° C., 400° C. or 450° C.; And / or, the calcination time is 10 h or 15 h.

21. A solid electrolyte, characterized in that: It is prepared according to the preparation method of the solid electrolyte according to any one of claims 1 to 20.

22. The solid electrolyte according to claim 21, characterized in that The cations in the solid electrolyte include Li ions and / or K ions; the anions in the solid electrolyte include one or more of Cl ions, Br ions, S ions and Se ions.

23. Use of the solid electrolyte according to claim 21 or 22 in preparing a battery.

24. An electrochemical device, characterized in that: It comprises the solid electrolyte as claimed in claim 21 or 22.

25. The electrochemical device according to claim 24, characterized in that The electrochemical device is a battery.

26. The electrochemical device according to claim 25, characterized in that The electrochemical device is a lithium ion battery.

Citation Information

Patent Citations

  • Molecular sieve supported sodium ion solid electrolyte and preparation method and application thereof

    CN111755734A

  • Composite solid electrolyte, lithium battery and preparation method

    CN116666737A

  • Metal battery with molecular sieve solid electrolyte layer

    CN106450512A

  • Preparation method of lithium borohydride-based solid electrolyte material

    CN109244535A

  • Lithium battery solid electrolyte based on MCM-41 molecular sieve solidified ionic liquid and preparation method thereof

    CN111740154A