Elastic cotton-like polyester fiber and preparation process thereof
Through the side-by-side compounding of PET and PBT materials and the modification of nano-mesoporous silica, the hygroscopic and antibacterial properties of polyester fiber are improved, the problems of insufficient comfort and water absorption performance of polyester fiber are solved, and more efficient fiber performance is achieved promote.
Patent Information
- Application Number
- CN202410295530.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Polyester fiber has poor performance in water absorption and perspiration performance, resulting in poor comfort. Natural cotton fiber resources are in short supply. It is necessary to improve the performance of polyester fiber to alleviate this problem.
PET and PBT materials are used for side-by-side composite spinning, and nanometer mesoporous silica is introduced during the fiber preparation process. Its antibacterial and hygroscopic properties are improved through acidification, oxidation and modification treatments, combined with bis(4-aminophenoxy)dioxide. Chemical substances such as methylsilane, isocyanate group and 4,5-diphenyl imidazolinone enhance the hydrophilicity and antibacterial activity of the fiber.
The mechanical strength, soaping resistance and friction resistance of elastic cotton-like polyester fiber are improved, while its hygroscopic and antibacterial properties are enhanced, improving wearing comfort.
Smart Images

Figure BDA0004742063370000111 
Figure BDA0004742063370000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fiber preparation, in particular to elastic cotton-like polyester fiber and a preparation process thereof. Background Art
[0002] In recent years, with the continuous development of my country's clothing fabric market, the textile industry has gradually faced the shortage of natural cotton fiber resources and soaring costs. On the other hand, polyester fiber is facing overcapacity. However, compared with natural cotton fiber, polyester fiber performs poorly in water absorption and other aspects, has poor perspiration function, and feels stuffy. Therefore, it is necessary to overcome these defects of polyester fiber to alleviate the shortage of natural cotton fiber and achieve efficient utilization of polyester fiber. Summary of the invention
[0003] The object of the present invention is to provide a stretch cotton-like polyester fiber and a preparation process thereof to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a preparation process of elastic cotton-like polyester fiber, comprising the following steps:
[0005] S1. Preparation of antibacterial nano-mesoporous silica;
[0006] S11. The nano-mesoporous silica is dispersed with nitric acid at a concentration of 50-60wt%, and subjected to ultrasonic dispersion treatment for 4-8h. The temperature is raised to 65-80°C, and the reaction is continued for 2-4h. The precipitate is separated by centrifugation, and washed with deionized water until neutral. After vacuum drying for 12-24h, the precipitate is dispersed again in DMF containing bis(4-aminophenoxy)dimethylsilane, and the temperature is raised to 80-95°C. After ultrasonic dispersion reaction for 8-10h, the aminated nano-mesoporous silica is obtained.
[0007] S12. The aminated nano-mesoporous silica was dispersed in DMAc, dibutyltin dilaurate was added, and the mixture was dispersed by ultrasonic mixing for 45-60 minutes, and then the mixture was added dropwise to a DMF solution in which isophorone diisocyanate was dispersed. The mixture was heated to 60-80°C under a nitrogen atmosphere, and the mixture was reacted for 2-4 hours. The mixture was centrifuged and precipitated. The precipitate was washed with DMF for 2-3 times, and then vacuum evaporated to a constant weight. The mixture was ground and dispersed to obtain isocyanate-aminated nano-mesoporous silica.
[0008] S13. Disperse 4,5-diphenylimidazolidinone in ethanol, mix for 10-15 minutes, add sodium hydroxide, heat to 55-60° C., stir and activate for 20-30 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0009] Mix 4-iodobenzyl alcohol and ethanol, add them dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere, heat to 72-75°C, reflux for 12-36 hours, remove excess solvent by rotary evaporation, wash the remaining product with tetrahydrofuran, collect the filtrate, and evaporate in vacuo to constant weight to obtain an imidazolinone benzyl alcohol compound;
[0010] S14. Dispersing the isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and subjecting the dispersion to ultrasonic dispersion for 2-4 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion;
[0011] Disperse the imidazolinone benzyl alcohol compound in tetrahydrofuran, heat it to 55-65°C, stir and disperse for 4-8h, then drop the isocyanate-modified nano-mesoporous silica dispersion, heat it to 45-60°C after the addition, stir and react for 2-4h, centrifuge and evaporate in vacuum to constant weight to obtain the isocyanate-modified nano-mesoporous silica;
[0012] S15. The lindole-modified nano-mesoporous silica was dispersed in acetone, trichloroisocyanuric acid was added, the temperature was raised to 45-60°C under a nitrogen atmosphere, the reaction was stirred for 4-8 hours, and the excess solvent was removed by rotary evaporation. The product was washed with n-hexane for 3-5 times, and then vacuum evaporated to constant weight to obtain antibacterial nano-mesoporous silica;
[0013] S2. PET and antibacterial nano-mesoporous silica are mixed and screw-melted, and PBT is dried and screw-melted; the screw-melted material is placed in a spinning manifold, and the spinning is performed in parallel and composited to prepare polyester fiber precursor;
[0014] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0015] Furthermore, in step S11, the mass ratio of the nano-mesoporous silica to bis(4-aminophenoxy)dimethylsilane is 5:(15-40) in parts by weight.
[0016] Furthermore, in step S12, the mass ratio of the amino-modified nano-mesoporous silica, dibutyltin dilaurate, and isophorone diisocyanate is 5:(0.1-0.5):(10-20).
[0017] Furthermore, in step S13, the mass ratio of the 4,5-diphenylimidazolidinone, sodium hydroxide and 4-iodobenzyl alcohol is 10:(1-1.7):(8.5-10).
[0018] Furthermore, in step S14, the mass ratio of the isocyanate-modified nano-mesoporous silica to the imidazolidinone benzyl alcohol compound is 5:(10-20).
[0019] Furthermore, in step S15, the mass ratio of the linolone-modified nano-mesoporous silica to trichloroisocyanuric acid is 5:(5-15).
[0020] Furthermore, in step S2, the mass ratio of PET, antibacterial nano-mesoporous silica, and PBT is 75:(2.5-4):(20-25).
[0021] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0022] 1. In order to improve the comfort of elastic cotton-like polyester fiber, the present application uses PET material and PBT material for parallel composite spinning to prepare elastic cotton-like polyester fiber. PET and PBT materials have good mechanical strength, excellent breaking strength and breaking elongation. Compared with natural cotton fiber, the elastic cotton-like polyester fiber prepared by the present invention is resistant to soap washing and friction, and has excellent wear resistance;
[0023] 2. In order to further enhance the hygroscopic properties of the elastic cotton-like polyester fiber, the present application also introduces nano-mesoporous silica material into the polyester fiber during the preparation process. The nano-mesoporous carbon dioxide material has a mesoporous structure and a large specific surface area, which can adsorb water vapor and reduce the stuffy feeling caused by sweating; and in order to enhance the antibacterial properties of the elastic cotton-like polyester fiber, the present application further modifies the nano-mesoporous silica material;
[0024] The present invention performs an acid oxidation treatment on nano-mesoporous silica, performs an oxidation treatment on the surface of the nano-mesoporous silica using nitric acid, grafts active groups such as carboxyl groups on the surface of the nano-mesoporous silica, and improves the reactivity of the material. On this basis, the present invention uses bis(4-aminophenoxy)dimethylsilane to further treat the nano-mesoporous silica, thereby introducing amino groups on the surface of the nano-mesoporous silica, and then reacts the nano-mesoporous silica with isophorone diisocyanate, thereby introducing free isocyanate groups on the surface of the nano-mesoporous silica.
[0025] Then, the present invention uses 4,5-diphenylimidazolidinone and 4-iodobenzyl alcohol as raw materials, utilizes iodine element to react with imine in 4,5-diphenylimidazolidinone, thereby introducing alcoholic hydroxyl group into 4,5-diphenylimidazolidinone, then mixes it with nano-mesoporous silica, utilizes the reaction between alcoholic hydroxyl group and isocyanate group, introduces 4,5-diphenylimidazolidinone on the surface of nano-mesoporous silica, then uses trichloroisocyanuric acid to react with it nucleophilically, introduces chlorine atom into 4,5-diphenylimidazolidinone, generates halogenamine structure with antibacterial activity, thereby making nano-mesoporous silica have antibacterial activity, and the introduction of halogenamine structure can further improve the hydrophilicity of nano-mesoporous silica material, improve the hygroscopicity of cotton-like polyester fiber, and improve wearing comfort. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The nano-mesoporous silica used in this application is XFF43 type 104015 hollow mesoporous silica produced by Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.; the bis(4-aminophenoxy)dimethylsilane used is provided by Shanghai Myrel Biochemical Technology Co., Ltd.; the 4,5-diphenylimidazolinone used is provided by Zhejiang Hangyu Pharmaceutical Technology Co., Ltd.; the 4-iodobenzyl alcohol used is provided by Shanghai Haohong Biopharmaceutical Technology Co., Ltd.; the PET used is WK-821 polyester chips produced by Zhejiang Wankai; the PBT chips used are produced by Polyplastics Co., Ltd. of Japan. 300FP PBT; the nano-silica used is XFF48 type 104437 nano-silica from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.;
[0028] Embodiment 1. A process for preparing elastic cotton-like polyester fiber, comprising the following steps:
[0029] S1. Preparation of antibacterial nano-mesoporous silica;
[0030] S11. By weight, 5 parts of nano-mesoporous silica were dispersed with 50wt% nitric acid, and subjected to ultrasonic dispersion for 4h. The temperature was raised to 65°C, and the reaction was continued for 2h. The precipitate was separated by centrifugation, and washed with deionized water until neutral. The precipitate was dried at 80°C in vacuum for 12h, and then dispersed again in DMF containing 15 parts of bis(4-aminophenoxy)dimethylsilane. The temperature was raised to 80°C, and the dispersion was subjected to ultrasonic dispersion for 8h to obtain amino-modified nano-mesoporous silica.
[0031] S12. Disperse 5 parts of amino-modified nano-mesoporous silica in DMAc by weight, add 0.1 parts of dibutyltin dilaurate, and add it dropwise to a DMF solution containing 10 parts of isophorone diisocyanate after ultrasonic mixing and dispersion for 45 minutes. Heat the mixture to 60°C under a nitrogen atmosphere, react for 2 hours, centrifuge and separate the precipitate. Wash the precipitate twice with DMF, evaporate it in vacuum to constant weight, grind and disperse it, and obtain isocyanate-modified nano-mesoporous silica.
[0032] S13. Disperse 10 parts of 4,5-diphenylimidazolidinone in ethanol by weight, mix for 10 minutes, add 1 part of sodium hydroxide, heat to 55 ° C, stir and activate for 20 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0033] 8.5 parts of 4-iodobenzyl alcohol was mixed with ethanol, and the mixture was added dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere. The mixture was heated to 72°C, and refluxed for 12 hours. The excess solvent was removed by rotary evaporation, and the remaining product was washed with tetrahydrofuran. The filtrate was collected and evaporated to constant weight under vacuum at 45°C to obtain an imidazolinone benzyl alcohol compound.
[0034] S14. Dispersing 5 parts of isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and ultrasonically dispersing for 2 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion;
[0035] Disperse 10 parts of imidazolinone benzyl alcohol compound in tetrahydrofuran, heat to 55°C, stir and disperse for 4 hours, then drop isocyanate-modified nano-mesoporous silica dispersion, heat to 45°C after the addition, stir and react for 2 hours, centrifuge, and evaporate in vacuo to constant weight to obtain imidazolinone-modified nano-mesoporous silica;
[0036] S15. Disperse 5 parts of phenoxyethylamine-modified nano-mesoporous silica in acetone by weight, add 5 parts of trichloroisocyanuric acid, heat to 45 ° C under nitrogen atmosphere, stir and react for 4 hours, remove excess solvent by rotary evaporation, wash the product 3 times with n-hexane, and evaporate to constant weight in vacuum to obtain antibacterial nano-mesoporous silica;
[0037] S2. By weight, 75 parts of PET and 2.5 parts of antibacterial nano-mesoporous silica were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was carried out in parallel composite to prepare polyester fiber precursor;
[0038] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0039] Embodiment 2. A process for preparing elastic cotton-like polyester fiber, comprising the following steps:
[0040] Compared with Example 1, this embodiment increases the amount of imidazolidinone benzyl alcohol compound added in step S14;
[0041] S1. Preparation of antibacterial nano-mesoporous silica;
[0042] S11. By weight, 5 parts of nano-mesoporous silica were dispersed with 50wt% nitric acid, and subjected to ultrasonic dispersion for 4h. The temperature was raised to 65°C, and the reaction was continued for 2h. The precipitate was separated by centrifugation, and washed with deionized water until neutral. The precipitate was dried at 80°C in vacuum for 12h, and then dispersed again in DMF containing 15 parts of bis(4-aminophenoxy)dimethylsilane. The temperature was raised to 80°C, and the dispersion was subjected to ultrasonic dispersion for 8h to obtain amino-modified nano-mesoporous silica.
[0043] S12. Disperse 5 parts of amino-modified nano-mesoporous silica in DMAc by weight, add 0.1 parts of dibutyltin dilaurate, and add it dropwise to a DMF solution containing 10 parts of isophorone diisocyanate after ultrasonic mixing and dispersion for 45 minutes. Heat the mixture to 60°C under a nitrogen atmosphere, react for 2 hours, centrifuge and separate the precipitate. Wash the precipitate twice with DMF, evaporate it in vacuum to constant weight, grind and disperse it, and obtain isocyanate-modified nano-mesoporous silica.
[0044] S13. Disperse 10 parts of 4,5-diphenylimidazolidinone in ethanol by weight, mix for 10 minutes, add 1 part of sodium hydroxide, heat to 55 ° C, stir and activate for 20 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0045] 8.5 parts of 4-iodobenzyl alcohol was mixed with ethanol, and the mixture was added dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere. The mixture was heated to 72°C, and refluxed for 12 hours. The excess solvent was removed by rotary evaporation, and the remaining product was washed with tetrahydrofuran. The filtrate was collected and evaporated to constant weight under vacuum at 45°C to obtain an imidazolinone benzyl alcohol compound.
[0046] S14. Dispersing 5 parts of isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and ultrasonically dispersing for 2 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion;
[0047] Disperse 20 parts of imidazolinone benzyl alcohol compound in tetrahydrofuran, heat to 55°C, stir and disperse for 4 hours, then drop isocyanate-modified nano-mesoporous silica dispersion, heat to 45°C after the addition, stir and react for 2 hours, centrifuge and evaporate in vacuo to constant weight to obtain imidazolinone-modified nano-mesoporous silica;
[0048] S15. Disperse 5 parts of phenoxyethylamine-modified nano-mesoporous silica in acetone by weight, add 5 parts of trichloroisocyanuric acid, heat to 45 ° C under nitrogen atmosphere, stir and react for 4 hours, remove excess solvent by rotary evaporation, wash the product 3 times with n-hexane, and evaporate to constant weight in vacuum to obtain antibacterial nano-mesoporous silica;
[0049] S2. By weight, 75 parts of PET and 2.5 parts of antibacterial nano-mesoporous silica were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was carried out in parallel composite to prepare polyester fiber precursor;
[0050] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0051] Embodiment 3. A process for preparing elastic cotton-like polyester fiber, comprising the following steps:
[0052] Compared with Example 2, this example increases the amount of isophorone diisocyanate added in step S12;
[0053] S1. Preparation of antibacterial nano-mesoporous silica;
[0054] S11. By weight, 5 parts of nano-mesoporous silica were dispersed with 50wt% nitric acid, and subjected to ultrasonic dispersion for 4h. The temperature was raised to 65°C, and the reaction was continued for 2h. The precipitate was separated by centrifugation, and washed with deionized water until neutral. The precipitate was dried at 80°C in vacuum for 12h, and then dispersed again in DMF containing 15 parts of bis(4-aminophenoxy)dimethylsilane. The temperature was raised to 80°C, and the dispersion was subjected to ultrasonic dispersion for 8h to obtain amino-modified nano-mesoporous silica.
[0055] S12. Disperse 5 parts of amino-modified nano-mesoporous silica in DMAc by weight, add 0.1 parts of dibutyltin dilaurate, and add it dropwise to a DMF solution containing 20 parts of isophorone diisocyanate after ultrasonic mixing and dispersion for 45 minutes. Heat to 60°C under nitrogen atmosphere, react for 2 hours, centrifuge and separate the precipitate. Wash the precipitate twice with DMF, evaporate it in vacuum to constant weight, grind and disperse it, and obtain isocyanate-modified nano-mesoporous silica.
[0056] S13. Disperse 10 parts of 4,5-diphenylimidazolidinone in ethanol by weight, mix for 10 minutes, add 1 part of sodium hydroxide, heat to 55 ° C, stir and activate for 20 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0057] 8.5 parts of 4-iodobenzyl alcohol was mixed with ethanol, and the mixture was added dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere. The mixture was heated to 72°C, and refluxed for 12 hours. The excess solvent was removed by rotary evaporation, and the remaining product was washed with tetrahydrofuran. The filtrate was collected and evaporated to constant weight under vacuum at 45°C to obtain an imidazolinone benzyl alcohol compound.
[0058] S14. Dispersing 5 parts of isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and ultrasonically dispersing for 2 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion;
[0059] Disperse 20 parts of imidazolinone benzyl alcohol compound in tetrahydrofuran, heat to 55°C, stir and disperse for 4 hours, then drop isocyanate-modified nano-mesoporous silica dispersion, heat to 45°C after the addition, stir and react for 2 hours, centrifuge and evaporate in vacuo to constant weight to obtain imidazolinone-modified nano-mesoporous silica;
[0060] S15. Disperse 5 parts of phenoxyethylamine-modified nano-mesoporous silica in acetone by weight, add 5 parts of trichloroisocyanuric acid, heat to 45 ° C under nitrogen atmosphere, stir and react for 4 hours, remove excess solvent by rotary evaporation, wash the product 3 times with n-hexane, and evaporate to constant weight in vacuum to obtain antibacterial nano-mesoporous silica;
[0061] S2. By weight, 75 parts of PET and 2.5 parts of antibacterial nano-mesoporous silica were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was carried out in parallel composite to prepare polyester fiber precursor;
[0062] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0063] Embodiment 4. A process for preparing a stretch cotton-like polyester fiber, comprising the following steps:
[0064] Compared with Example 2, this example increases the amount of 4-iodobenzyl alcohol added in step S13;
[0065] S1. Preparation of antibacterial nano-mesoporous silica;
[0066] S11. By weight, 5 parts of nano-mesoporous silica were dispersed with 50wt% nitric acid, and subjected to ultrasonic dispersion for 4h. The temperature was raised to 65°C, and the reaction was continued for 2h. The precipitate was separated by centrifugation, and washed with deionized water until neutral. The precipitate was dried at 80°C in vacuum for 12h, and then dispersed again in DMF containing 15 parts of bis(4-aminophenoxy)dimethylsilane. The temperature was raised to 80°C, and the dispersion was subjected to ultrasonic dispersion for 8h to obtain amino-modified nano-mesoporous silica.
[0067] S12. Disperse 5 parts of amino-modified nano-mesoporous silica in DMAc by weight, add 0.1 parts of dibutyltin dilaurate, and add it dropwise to a DMF solution containing 10 parts of isophorone diisocyanate after ultrasonic mixing and dispersion for 45 minutes. Heat the mixture to 60°C under a nitrogen atmosphere, react for 2 hours, centrifuge and separate the precipitate. Wash the precipitate twice with DMF, evaporate it in vacuum to constant weight, grind and disperse it, and obtain isocyanate-modified nano-mesoporous silica.
[0068] S13. Disperse 10 parts of 4,5-diphenylimidazolidinone in ethanol by weight, mix for 10 minutes, add 1 part of sodium hydroxide, heat to 55 ° C, stir and activate for 20 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0069] 10 parts of 4-iodobenzyl alcohol and ethanol were mixed, and the mixture was added dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere, and the mixture was heated to 72°C. After reflux reaction for 12 hours, the excess solvent was removed by rotary evaporation, and the remaining product was washed with tetrahydrofuran. The filtrate was collected and evaporated to constant weight at 45°C in vacuum to obtain an imidazolinone benzyl alcohol compound;
[0070] S14. Dispersing 5 parts of isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and ultrasonically dispersing for 2 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion;
[0071] Disperse 20 parts of imidazolinone benzyl alcohol compound in tetrahydrofuran, heat to 55°C, stir and disperse for 4 hours, then drop isocyanate-modified nano-mesoporous silica dispersion, heat to 45°C after the addition, stir and react for 2 hours, centrifuge and evaporate in vacuo to constant weight to obtain imidazolinone-modified nano-mesoporous silica;
[0072] S15. Disperse 5 parts of phenoxyethylamine-modified nano-mesoporous silica in acetone by weight, add 5 parts of trichloroisocyanuric acid, heat to 45 ° C under nitrogen atmosphere, stir and react for 4 hours, remove excess solvent by rotary evaporation, wash the product 3 times with n-hexane, and evaporate to constant weight in vacuum to obtain antibacterial nano-mesoporous silica;
[0073] S2. By weight, 75 parts of PET and 2.5 parts of antibacterial nano-mesoporous silica were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was carried out in parallel composite to prepare polyester fiber precursor;
[0074] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0075] Embodiment 5. A process for preparing a stretch cotton-like polyester fiber, comprising the following steps:
[0076] Compared with Example 2, this example increases the amount of antibacterial nano-mesoporous silica added in step S2;
[0077] S1. Preparation of antibacterial nano-mesoporous silica;
[0078] S11. By weight, 5 parts of nano-mesoporous silica were dispersed with 50wt% nitric acid, and subjected to ultrasonic dispersion for 4h. The temperature was raised to 65°C, and the reaction was continued for 2h. The precipitate was separated by centrifugation, and washed with deionized water until neutral. The precipitate was dried at 80°C in vacuum for 12h, and then dispersed again in DMF containing 15 parts of bis(4-aminophenoxy)dimethylsilane. The temperature was raised to 80°C, and the dispersion was subjected to ultrasonic dispersion for 8h to obtain amino-modified nano-mesoporous silica.
[0079] S12. Disperse 5 parts of amino-modified nano-mesoporous silica in DMAc by weight, add 0.1 parts of dibutyltin dilaurate, and add it dropwise to a DMF solution containing 10 parts of isophorone diisocyanate after ultrasonic mixing and dispersion for 45 minutes. Heat the mixture to 60°C under a nitrogen atmosphere, react for 2 hours, centrifuge and separate the precipitate. Wash the precipitate twice with DMF, evaporate it in vacuum to constant weight, grind and disperse it, and obtain isocyanate-modified nano-mesoporous silica.
[0080] S13. Disperse 10 parts of 4,5-diphenylimidazolidinone in ethanol by weight, mix for 10 minutes, add 1 part of sodium hydroxide, heat to 55 ° C, stir and activate for 20 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0081] 8.5 parts of 4-iodobenzyl alcohol was mixed with ethanol, and the mixture was added dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere. The mixture was heated to 72°C, and refluxed for 12 hours. The excess solvent was removed by rotary evaporation, and the remaining product was washed with tetrahydrofuran. The filtrate was collected and evaporated to constant weight under vacuum at 45°C to obtain an imidazolinone benzyl alcohol compound.
[0082] S14. Dispersing 5 parts of isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and ultrasonically dispersing for 2 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion;
[0083] Disperse 20 parts of imidazolinone benzyl alcohol compound in tetrahydrofuran, heat to 55°C, stir and disperse for 4 hours, then drop isocyanate-modified nano-mesoporous silica dispersion, heat to 45°C after the addition, stir and react for 2 hours, centrifuge and evaporate in vacuo to constant weight to obtain imidazolinone-modified nano-mesoporous silica;
[0084] S15. Disperse 5 parts of phenoxyethylamine-modified nano-mesoporous silica in acetone by weight, add 5 parts of trichloroisocyanuric acid, heat to 45 ° C under nitrogen atmosphere, stir and react for 4 hours, remove excess solvent by rotary evaporation, wash the product 3 times with n-hexane, and evaporate to constant weight in vacuum to obtain antibacterial nano-mesoporous silica;
[0085] S2. By weight, 75 parts of PET and 4 parts of antibacterial nano-mesoporous silica were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was carried out in parallel composite to prepare polyester fiber precursor;
[0086] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0087] Comparative Example 1. A process for preparing elastic cotton-like polyester fiber, comprising the following steps:
[0088] Compared with Example 2, this comparative example did not prepare antibacterial nano-mesoporous silica, but only used nano-mesoporous silica;
[0089] S2. By weight, 75 parts of PET and 2.5 parts of nano-mesoporous silica were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was performed in parallel and compounded to prepare polyester fiber precursor;
[0090] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0091] Comparative Example 2. A process for preparing a stretch cotton-like polyester fiber, comprising the following steps:
[0092] Compared with Example 2, this comparative example uses nano-silica to replace nano-mesoporous silica;
[0093] S1. Preparation of antibacterial nano-silica;
[0094] S11. By weight, 5 parts of nano-silicon dioxide were dispersed with 50wt% nitric acid, and subjected to ultrasonic dispersion for 4h. The temperature was raised to 65°C, and the reaction was continued for 2h. The precipitate was separated by centrifugation, washed with deionized water until neutral, and dried at 80°C in vacuum for 12h. The precipitate was dispersed again in DMF containing 15 parts of bis(4-aminophenoxy)dimethylsilane, and the temperature was raised to 80°C. After ultrasonic dispersion for 8h, the aminated nano-silicon dioxide was obtained.
[0095] S12. Disperse 5 parts of amino-modified nano-silica in DMAc by weight, add 0.1 parts of dibutyltin dilaurate, and disperse by ultrasonic mixing for 45 minutes, then add it dropwise to a DMF solution containing 10 parts of isophorone diisocyanate, heat to 60°C under a nitrogen atmosphere, react for 2 hours, centrifuge and separate the precipitate, wash the precipitate twice with DMF, evaporate in vacuo to constant weight, grind and disperse, and obtain isocyanate-modified nano-silica;
[0096] S13. Disperse 10 parts of 4,5-diphenylimidazolidinone in ethanol by weight, mix for 10 minutes, add 1 part of sodium hydroxide, heat to 55 ° C, stir and activate for 20 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion;
[0097] 8.5 parts of 4-iodobenzyl alcohol was mixed with ethanol, and the mixture was added dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere. The mixture was heated to 72°C, and refluxed for 12 hours. The excess solvent was removed by rotary evaporation, and the remaining product was washed with tetrahydrofuran. The filtrate was collected and evaporated to constant weight under vacuum at 45°C to obtain an imidazolinone benzyl alcohol compound.
[0098] S14. In parts by weight, 5 parts of isocyanate-based nano-silica were dispersed in tetrahydrofuran, and ultrasonically dispersed for 2 hours to obtain an isocyanate-based nano-silica dispersion;
[0099] Disperse 20 parts of imidazolinone benzyl alcohol compound in tetrahydrofuran, heat to 55°C, stir and disperse for 4 hours, then drop isocyanate-modified nano-silica dispersion, heat to 45°C after the addition, stir and react for 2 hours, centrifuge, and evaporate in vacuo to constant weight to obtain imidazolinone-modified nano-silica;
[0100] S15. Disperse 5 parts of phenoxyethyl ketone-modified nano-silica in acetone by weight, add 5 parts of trichloroisocyanuric acid, heat to 45 ° C under nitrogen atmosphere, stir and react for 4 hours, remove excess solvent by rotary evaporation, wash the product 3 times with n-hexane, and evaporate to constant weight in vacuum to obtain antibacterial nano-silica;
[0101] S2. By weight, 75 parts of PET and 2.5 parts of antibacterial nano-silicon dioxide were mixed, and the temperature of the screw melting zone 1 was 285°C, the temperature of the screw melting zone 2 was 284°C, the temperature of the screw melting zone 3 was 283°C, the temperature of the screw melting zone 4 was 283°C, the temperature of the screw melting zone 5 was 282°C, and the temperature of the screw melting zone 6 was 270°C; 20 parts of PBT were melted, and the temperature of the screw melting zone 1 was 259°C, the temperature of the screw melting zone 2 was 265.5°C, the temperature of the screw melting zone 3 was 269.3°C, the temperature of the screw melting zone 4 was 270.3°C, and the temperature of the screw melting zone 5 was 271.3°C; the above-mentioned screw melted materials were placed in a spinning manifold, and the spinning was performed in parallel and compounded to prepare polyester fiber precursor;
[0102] S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
[0103] Testing: The elastic cotton-like polyester fibers prepared in Examples 1-5 and Comparative Examples 1-2 were prepared into fiber materials with a fineness of 1.25±0.02 dtex, and woven into 32S polyester plain weave fabrics. The water absorption was tested according to GB / T 21665.1-2008. According to GB 15979-2002, the antibacterial properties of the polyester plain weave fabrics against Escherichia coli and Staphylococcus aureus were tested by the film culture method. According to GB / T 14337-2022, the mechanical properties of the single polyester fiber yarns were tested by using a fiber strength and elongation tester, with a test tension of 0.15 cN / dtex, a stretching rate of 20 mm / min, a traction multiple of 1.6 times, and a clamping distance of 20 mm.
[0104] The test results are shown in the table below;
[0105]
[0106]
[0107] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing elastic cotton-like polyester fiber, characterized in that: The following steps are involved: S1. Preparation of antibacterial nano-mesoporous silica; S11. The nano-mesoporous silica is dispersed with nitric acid at a concentration of 50-60wt%, and subjected to ultrasonic dispersion treatment for 4-8h. The temperature is raised to 65-80°C, and the reaction is continued for 2-4h. The precipitate is separated by centrifugation, and washed with deionized water until neutral. After vacuum drying for 12-24h, the precipitate is dispersed again in DMF containing bis(4-aminophenoxy)dimethylsilane, and the temperature is raised to 80-95°C. After ultrasonic dispersion reaction for 8-10h, the aminated nano-mesoporous silica is obtained. Wherein, the mass ratio of the nano-mesoporous silica to bis(4-aminophenoxy)dimethylsilane is 5:(15-40); S12. The aminated nano-mesoporous silica was dispersed in DMAc, dibutyltin dilaurate was added, and the mixture was dispersed by ultrasonic mixing for 45-60 minutes, and then the mixture was added dropwise to a DMF solution in which isophorone diisocyanate was dispersed. The mixture was heated to 60-80°C under a nitrogen atmosphere, and the mixture was reacted for 2-4 hours. The mixture was centrifuged and precipitated. The precipitate was washed with DMF for 2-3 times, and then vacuum evaporated to a constant weight. The mixture was ground and dispersed to obtain isocyanate-aminated nano-mesoporous silica. Wherein, the mass ratio of the amino-modified nano-mesoporous silica, dibutyltin dilaurate, and isophorone diisocyanate is 5:(0.1-0.5):(10-20); S13. Disperse 4,5-diphenylimidazolidinone in ethanol, mix for 10-15 minutes, add sodium hydroxide, heat to 55-60° C., stir and activate for 20-30 minutes, and cool to room temperature to obtain a 4,5-diphenylimidazolidinone dispersion; Mix 4-iodobenzyl alcohol and ethanol, add them dropwise to the 4,5-diphenylimidazolinone dispersion under a nitrogen atmosphere, heat to 72-75°C, reflux for 12-36 hours, remove excess solvent by rotary evaporation, wash the remaining product with tetrahydrofuran, collect the filtrate, and evaporate in vacuo to constant weight to obtain an imidazolinone benzyl alcohol compound; Wherein, the mass ratio of 4,5-diphenylimidazolidinone, sodium hydroxide and 4-iodobenzyl alcohol is 10:(1-1.7):(8.5-10); S14. Dispersing the isocyanate-modified nano-mesoporous silica in tetrahydrofuran, and subjecting the dispersion to ultrasonic dispersion for 2-4 hours to obtain an isocyanate-modified nano-mesoporous silica dispersion; Disperse the imidazolinone benzyl alcohol compound in tetrahydrofuran, heat it to 55-65°C, stir and disperse for 4-8h, then drop the isocyanate-modified nano-mesoporous silica dispersion, heat it to 45-60°C after the addition, stir and react for 2-4h, centrifuge and evaporate in vacuum to constant weight to obtain the isocyanate-modified nano-mesoporous silica; Wherein, the mass ratio of the isocyanate-modified nano-mesoporous silica to the imidazolinone benzyl alcohol compound is 5:(10-20); S15. The lindole-modified nano-mesoporous silica was dispersed in acetone, trichloroisocyanuric acid was added, the temperature was raised to 45-60°C under a nitrogen atmosphere, the reaction was stirred for 4-8 hours, and the excess solvent was removed by rotary evaporation. The product was washed with n-hexane for 3-5 times, and then vacuum evaporated to constant weight to obtain antibacterial nano-mesoporous silica; Wherein, the mass ratio of the linolone-modified nano-mesoporous silica to trichloroisocyanuric acid is 5:(5-15); S2. PET and antibacterial nano-mesoporous silica are mixed and screw-melted, and PBT is dried and screw-melted; the screw-melted material is placed in a spinning manifold, and the spinning is performed in parallel and composited to prepare polyester fiber precursor; S3. The polyester fiber raw yarn is wound and oiled, and then stretched, curled and shaped to obtain elastic cotton-like polyester fiber.
2. The process for preparing the elastic cotton-like polyester fiber according to claim 1, characterized in that: In step S2, the mass ratio of PET, antibacterial nano-mesoporous silica, and PBT is 75: (2.5-4):(20-25)。 3. An elastic cotton-like polyester fiber prepared by the preparation process according to any one of claims 1 to 2.
Citation Information
Patent Citations
Antibacterial, moisture absorption and sweat releasing polyester composite elastic fiber
CN104726947A
Preparation method of bi-component fibers
CN111041568A