Difficult-to-graphitize carbon, negative electrode for lithium-ion secondary batteries and lithium-ion secondary batteries
By controlling the Guinier radius and pore structure of difficult-graphitizable carbon, the problem of insufficient discharge capacity in lithium-ion secondary batteries is solved, efficient battery performance improvement is achieved, and it is suitable for stable power storage of ESS.
Patent Information
- Application Number
- CN202380013945.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-26
AI Technical Summary
It is difficult for existing carbon materials to achieve high discharge capacity and stable cycle characteristics in lithium-ion secondary batteries. Especially in ESS applications, it is difficult to independently control the average particle size and specific surface area, resulting in insufficient discharge capacity.
Through small-angle X-ray scattering measurement and Guinier analysis, the Guinier radii Rg1 and Rg2 of difficult-graphitizable carbon are controlled within a specific range, and the particle size, shape and pore structure are adjusted by combining cross-linking, non-melting and sintering treatments. , ensuring high discharge capacity and charge and discharge efficiency of electrode materials.
It achieves high discharge capacity and excellent charge and discharge efficiency of the lithium-ion secondary battery negative electrode, meeting the stability and high volume capacity requirements of ESS.
Smart Images

Figure CN118076559B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to hardly graphitizable carbon, a negative electrode for a lithium ion secondary battery and a lithium ion secondary battery. Background Art
[0002] In recent years, due to the improvement of global awareness of the protection of the earth's environment, in order to reduce the use of fossil fuels and reduce CO2 emissions, power generation using renewable energy has gradually become popular. Renewable energy generated by solar power generation, wind power generation, etc. is easily affected by time period, season, climate, etc. Therefore, by making full use of the energy storage system (Energy Storage System, hereinafter referred to as "ESS") for suppressing output fluctuations, the stabilization of power supply can be achieved. Since large-scale batteries are required for the energy storage system, lithium-ion secondary batteries (LIBs) with high energy density per unit volume and mass and capable of miniaturization have attracted much attention. At present, carbon materials are generally used as negative electrode materials for lithium-ion secondary batteries. In addition to carbon, lithium salts of metals or metal oxides such as Si, Sn, Ti, V, etc., and mixed materials of carbon and metals with high energy density are in the research stage.
[0003] Among carbon materials, graphite materials are widely used in portable electronic devices because they generally have high capacity. For ESS applications, non-graphitizable carbon materials with high charge-discharge capacity and cycle characteristics are suitable. In particular, unlike batteries for hybrid vehicles, ESS applications strongly require high discharge capacity, high volume capacity for miniaturization, and life characteristics that allow for repeated charge and discharge for a long time.
[0004] Regarding the difficult-to-graphitize carbon material as the negative electrode material of the lithium-ion secondary battery, it is characterized by being formed by non-oriented graphene layer units, having a high c-axis length and a small crystallite diameter compared to graphite materials, and having pores between the graphene layer units. Due to these structural features, Li can be absorbed not only between layers but also in pores. Therefore, it can be seen that compared with the theoretical capacity of graphite 372mAh / g, the difficult-to-graphitize carbon has a higher discharge capacity. In addition, due to the long c-axis length, the volume change accompanying the insertion / extraction of Li is also small, and the life characteristics are also excellent.
[0005] Regarding non-graphitizable carbon, for example, Patent Document 1 discloses that the scattering intensity I of the small-angle X-ray scattering of the carbonaceous material is S(0) By setting the concentration to a specific range, a secondary battery having a high doping-dedoping amount can be obtained (claim 1, paragraphs 0008 and 0019).
[0006] Patent document 2 discloses a carbonaceous material having an average particle size, specific surface area, etc. set within a specific range as a carbonaceous material for a negative electrode of a non-aqueous electrolyte secondary battery that exhibits good charge and discharge capacity and low resistance in automotive applications and has good resistance to oxidative degradation (claim 1, paragraphs 0006 and 0007).
[0007] Patent Document 3 defines the slope A of the scattering intensity in a specific wavenumber range in a small-angle X-ray scattering spectrum, etc. for a carbon material used as a negative electrode of a sodium secondary battery (paragraphs 0079, 0100 to 0107).
[0008] Regarding the preparation of carbon materials, Patent Document 4 discloses a carbon material for a negative electrode of a non-aqueous solvent secondary battery, which is prepared by modifying a precursor asphalt or tar obtained by polymerizing condensed polycyclic hydrocarbons or substances containing them in the presence of hydrogen fluoride / boron trifluoride, subjecting the modified asphalt with 100% optical isotropy to an infusibility treatment and then calcining the modified asphalt.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 7-320740
[0012] Patent Document 2: Japanese Patent No. 6245412
[0013] Patent Document 3: International Publication No. 2014 / 157125
[0014] Patent Document 4: Japanese Patent Application Laid-Open No. 10-083814 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, the carbon material of Patent Document 1 focuses on the scattering vector q of 0.1256 nm. -1 To 0.2083nm -1 The vertical axis intercept of the Guinier plot is within the range of , and the high discharge capacity required for ESS applications cannot be obtained.
[0017] The carbon material of Patent Document 2 also requires properties for vehicle use, and cannot obtain sufficient discharge capacity when used for ESS. In addition, the average particle size and specific surface area cannot be independently controlled, so it is difficult to set them to specific ranges, and the properties may change depending on the shape of the particles.
[0018] The carbon material of Patent Document 3 relates to a sodium ion secondary battery, and only controls the scattering vector q of the described small-angle X-ray scattering to 0.6 nm. -1 To 1.8nm -1 The slope of the non-Guinier plot in the wave number range of 200 Å is close to a straight line, which makes it difficult to obtain a high discharge capacity in a lithium ion secondary battery.
[0019] The carbon material of Patent Document 4 cannot achieve the high discharge capacity required for ESS applications.
[0020] Therefore, an object of the present invention is to provide a non-graphitizable carbon having a high discharge capacity, a negative electrode for a lithium ion secondary battery, and a lithium ion secondary battery.
[0021] Solution to the problem
[0022] The present inventors have conducted intensive research on a non-graphitizable carbon material having a high discharge capacity in order to solve the above-mentioned problems. As a result, it has been shown that non-graphitizable carbon having a given structure has a high discharge capacity.
[0023] The present invention is based on the above findings, and specifically, solves the above problems by employing the following configuration.
[0024] That is, the present invention provides the following [1] to [5].
[0025] [1] A non-graphitizable carbon having a scattering vector q of 0.30 nm obtained by small-angle X-ray scattering measurement and Guinier analysis. -1 Above and 0.40nm -1 The following range of the Guinier radius Rg1 is 3.00 nm or more and 5.80 nm or less,
[0026] The scattering vector q is 2.05nm -1 Above and 2.85nm -1 The following range of the Guinier radius Rg2 is 0.35 nm or more and 0.57 nm or less, and
[0027] The non-graphitizable carbon has an average interplanar spacing d002 of (002) planes determined by X-ray diffraction of 0.365 nm or more and 0.375 nm or less.
[0028] [2] The non-graphitizable carbon according to [1], wherein the average particle size is 20 μm or more and 40 μm or less.
[0029] [3] The non-graphitizable carbon according to [1] or [2], wherein the true specific gravity is 1.45 or more and 1.58 or less.
[0030] [4] A negative electrode for a lithium ion secondary battery, comprising the hardly graphitizable carbon according to any one of [1] to [3].
[0031] [5] A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to [4].
[0032] Effects of the Invention
[0033] According to the present invention, it is possible to provide hardly graphitizable carbon having a high discharge capacity, a negative electrode for a lithium ion secondary battery, and a lithium ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Graph showing the relationship between the natural logarithm of the scattering intensity Δintensity of the non-graphitizable carbon of Example 4 and Comparative Example 3 and the square of the scattering vector q.
[0035] Figure 2 This is a cross-sectional view of an evaluation battery produced to evaluate battery characteristics in Examples and Comparative Examples.
[0036] Explanation of symbols
[0037] 1: External cup
[0038] 2: Working electrode (negative electrode)
[0039] 3: External can
[0040] 4: Counter electrode (positive electrode)
[0041] 5: Partition
[0042] 6: Insulation pad
[0043] 7a: Current Collector
[0044] 7b: Current collector DETAILED DESCRIPTION
[0045] In this specification, when "to" is used to express a range, the range includes both ends of "to". For example, a range such as A to B includes A and B.
[0046] [Difficult to graphitize carbon]
[0047] The hardly graphitizable carbon of the present invention (the carbon of the present invention) is a hardly graphitizable carbon having a scattering vector q of 0.30 nm obtained by small-angle X-ray scattering measurement and Guinier analysis. -1 Above and 0.40nm -1 The following range of the Guinier radius Rg1 is 3.00 nm or more and 5.80 nm or less,
[0048] The above scattering vector q is 2.05nm -1 Above and 2.85nm -1The following range of Guinier radius Rg2 is 0.35nm or more and 0.57nm or less, and
[0049] The average interplanar spacing d002 of the (002) plane determined by X-ray diffraction is 0.365 nm or more and 0.375 nm or less.
[0050] <Small-angle X-ray scattering>
[0051] 《Guignier radius Rg1》
[0052] Generally, when particles are used as samples, the scattering intensity obtained by small-angle X-ray scattering analysis is obtained by superposition of scattering from a plurality of pores in the particles and the surface shape of the particles.
[0053] In addition, the range of the scattering vector q is 0.30nm -1 Above and 0.40nm -1 The scattering at the following time is mainly obtained by scattering from the particle surface shape. The Guinier radius Rg1 (hereinafter also referred to as "Rg1") obtained by Guinier analysis within the range of the above-mentioned scattering vector q includes information such as particle size, particle shape, specific surface area, pores on the surface of the particle, and roughness of the particle. When the particle size is large, the specific surface area is small, the pores on the surface are small, and the roughness of the particle is small, Rg1 tends to become smaller.
[0054] The scattering vector q is expressed by the following equation.
[0055] Scattering vector q = 4πsinθ / λ (θ: scattering angle, λ: wavelength of X-ray)
[0056] The carbon of the present invention has an Rg1 of 3.00 nm or more and 5.80 nm or less, and thus has a particle shape most suitable for producing an electrode (particularly a negative electrode), can obtain a high discharge capacity, and is excellent in charge and discharge efficiency.
[0057] When Rg1 is less than 3.00 nm, the particle size is too large or the particle surface becomes smooth, making it difficult to apply the electrode. When Rg1 exceeds 5.80 nm, the particle size is too small or the surface area of the particle increases, making it impossible to apply the electrode thicker. In addition, the reaction area on the particle surface increases, reducing the charge and discharge efficiency.
[0058] From the viewpoint of obtaining a higher discharge capacity and excellent charge and discharge efficiency, Rg1 is preferably 4.20 nm or more.
[0059] From the viewpoint of maintaining the charge and discharge efficiency, Rg1 is preferably 5.70 nm or less.
[0060] Control of Rg1
[0061] As a control of Rg1, for example, by subjecting the raw material of the difficult-graphitizing carbon to a cross-linking treatment and an infusible treatment to obtain an infusible product, the infusible product is pulverized and fired to adjust the particle size, particle shape, specific surface area, surface roughness, etc., thereby Rg1 can be controlled to the above-mentioned given range. In particular, by setting the infusibility to a multi-step process to uniformize the degree of oxidation inside the particles, the Guinier radius Rg1 of the present invention can be controlled to a given range. In addition, by adjusting the pulverization conditions and removing unnecessary fine powders, coarse powders, and particles of special shapes from the difficult-graphitizing carbon after the pulverization as needed, or mixing two or more difficult-graphitizing carbons pulverized under their respective pulverization conditions, the Guinier radius Rg1 of the present invention can also be controlled to a given range.
[0062] 《Guignier radius Rg2》
[0063] Usually, particles are used as samples and small angle X-ray scattering analysis is performed, and the range of the scattering vector q is 2.05nm -1 Above and 2.85nm -1 The scattering at the following time is mainly obtained by scattering from the pores in the particle. The Guinier radius Rg2 (hereinafter also referred to as "Rg2") obtained by Guinier analysis within the range of the above scattering vector q contains information about the size of the pores in the particle. In the present invention, Rg2 is equivalent to the inertia radius of the pores present in the non-graphitizable carbon.
[0064] Since Rg2 is 0.35 nm or more and 0.57 nm or less, the carbon of the present invention has a large number of pores that are most suitable for absorbing and releasing Li during charge and discharge, and can obtain a high discharge capacity, and is excellent in discharge capacity and charge and discharge efficiency.
[0065] When Rg2 exceeds 0.57nm, the charge and discharge efficiency is excellent due to the presence of many large pores, but the pores of the size that can replenish Li are small and the discharge capacity becomes small. When Rg2 is less than 0.35nm, the pores of the size that can replenish Li become more and the charge capacity is excellent, but the replenished Li becomes difficult to release and the charging efficiency decreases.
[0066] From the perspective of obtaining a higher discharge capacity and excellent charge and discharge efficiency, Rg2 is preferably not less than 0.38 nm and not more than 0.50 nm.
[0067] ·Rg2 control
[0068] As the control of Rg2, for example, when the raw material of the difficult graphitizable carbon is cross-linked, infusible, pulverized, or sintered, in particular, by making the infusibility a multi-step process, the degree of oxidation inside the particles is uniform, so that Rg2 can be controlled to be within the above-mentioned given range. In addition, by setting the sintering temperature to 600 to 850° C., Rg2 that is effective for the absorption and release of Li can be controlled. In addition, in addition to the above-mentioned treatment, Rg2 can also be controlled by alkali treatment, etc. From the viewpoint of cost, Rg2 is preferably controlled by the sintering temperature.
[0069] Calculation of Guinier radius Rg1 and Rg2
[0070] Regarding the carbon of the present invention, the Guinier radii Rg1 and Rg2 can be obtained by small-angle X-ray scattering. The Guinier radii Rg1 and Rg2 can be calculated by measuring small-angle X-ray scattering and performing Guinier analysis as follows.
[0071] The measurement of small-angle X-ray scattering was performed under the following conditions.
[0072] Beamline: Spring8 BL08 B2-SAXS
[0073] Energy: 12.4keV
[0074] Detector: PILATUS3-S-1M
[0075] Camera constant (camera length) 2 horizontal measurement camera constant: 558mm
[0076] Small angle X-ray scattering measurements were performed according to the following procedures.
[0077] The scattering of the sample placed in the capillary is measured, and the two-dimensional data is converted into one dimension by circumferential averaging, and the scattering vector q (nm -1 ), i.e., the scattering intensity Int. sample In addition, the scattering of only the capillary was measured, and the two-dimensional data was converted into one dimension by circumferential averaging, and the scattering vector q (nm -1 ), namely the scattering intensity Int. blank .
[0078] The transmittance T of the sample is calculated by the following formula (1): sample The transmittance T of the capillary tube alone is obtained by the following formula (2): blank Here, the parameters in equations (1) and (2) are as follows. It should be noted that the incident X-ray intensity is measured in the ion chamber upstream of the sample, and the transmitted X-ray intensity is measured by the PIN diode of the beam stopper downstream of the sample.
[0079] I0sample : Incident X-ray intensity of capillary + sample
[0080] I 1sample : Transmitted X-ray intensity of capillary + sample
[0081] I 0blank : Incident X-ray intensity of the capillary only
[0082] I 1blank : Transmitted X-ray intensity of the capillary only
[0083] I 0air : Incident X-ray intensity of air only
[0084] I 1air : Transmitted X-ray intensity of air only
[0085] I 0dark : Dark current of the ion chamber
[0086] I 1dark : Dark current of PIN diode
[0087] [Mathematical formula 1]
[0088]
[0089]
[0090] Furthermore, the scattered intensity Δintensity from the sample was calculated using the following formula.
[0091] Δintensity=Int. sample / T sample -Int. blank / T blank
[0092] The scattered intensity from the sample Δ intensity The function of the scattering vector q can be used to calculate the Guinier radius Rg1 and Rg2 by performing Guinier analysis. 2 The method of calculating the Guinier radius based on the slope of the straight line area is used to draw a graph. The range of the scattering vector q is 0.30nm -1 Above and 0.40nm -1 The following slope is equivalent to -1 / 3Rg1 2 , scattering vector q range 2.05nm -1 Above and 2.85nm -1 The following slope is equivalent to -1 / 3Rg2 2 Thus, the Guinier radii Rg1 and Rg2 can be obtained.
[0093] Figure 1 (a) and (b) show examples of Guinier analysis of Example 4 and Comparative Example 3.
[0094] Figure 1 (a) and (b) are graphs (charts) showing the relationship between the natural logarithm of the scattering intensity Δintensity and the square of the scattering vector q of Example 4 and Comparative Example 3. Figure 1 In (a) and (b), the vertical axis of the graph represents lnΔintensity, and the horizontal axis of the graph represents q 2 In each graph, as indicated by arrows, the dotted line represents Example 4, and the solid line represents Comparative Example 3.
[0095] exist Figure 1 In (a), the scattering vector q is 0.30 nm. -1 Above and 0.40nm -1 Below (the square of the scattering vector q is 0.09nm -2 Above and 0.16nm -2 In the range of 20° (hereinafter referred to as 20°), a straight line region is obtained for Example 4, and the Guinier radius Rg1 of Example 4 can be obtained from the slope of the straight line in the above range. The Guinier radius Rg1 of Comparative Example 3 can also be obtained in the same manner as above.
[0096] exist Figure 1 In (b), the scattering vector q is 2.05 nm. -1 Above and 2.85nm -1 Below (the square of the scattering vector q is 4.20nm -2 Above and 8.12nm -2 In the range of (below), a straight line region is obtained for Example 4, and the Guinier radius Rg2 of Example 4 can be obtained based on the slope of the straight line in the above range. The Guinier radius Rg2 of Comparative Example 3 can also be obtained in the same manner as above.
[0097] <Average interplanar spacing d002 of (002) plane>
[0098] The average interplanar spacing d002 of the (002) plane in X-ray diffraction of the non-graphitizable carbon of the present invention (hereinafter, also simply referred to as “average interplanar spacing d002”) is 0.365 nm or more and 0.375 nm or less.
[0099] When the average interplanar spacing d002 is less than 0.365nm, the insertion / extraction opening of Li is small and it is difficult to insert / extract, and the discharge capacity is reduced. In addition, with the insertion / extraction of Li, the average interplanar spacing d002 repeatedly expands and shrinks, the crystal structure is destroyed, and the cycle life is reduced. When the average interplanar spacing d002 exceeds 0.375nm, the volume capacity is reduced.
[0100] From the perspective of being able to obtain a higher discharge capacity and maintain a cycle life or volume capacity, the average interplanar spacing d002 is preferably not less than 0.370 nm and not more than 0.374 nm.
[0101] Control of average interplanar spacing d002
[0102] The method for controlling the average interplanar spacing d002 is not particularly limited. For example, as a raw material for non-graphitizable carbon, a raw material can be selected that makes the average interplanar spacing d002 reach a given range by calcining it. Such a raw material can be selected from asphalts such as coal-based asphalt and petroleum-based asphalt; resins such as phenolic resin and furan resin; mixtures of asphalt and resin; etc., and in the case of coal-based asphalt, the average interplanar spacing d002 is easy to reach a given range, so it is preferred.
[0103] Determination of average interplanar spacing d002
[0104] In the present invention, the average interplanar spacing d002 is calculated based on the position of the peak by measuring the diffraction peak of the (002) plane of non-graphitizable carbon using CuKα line as X-ray and high-purity silicon as standard material. The calculation method is in accordance with the Gakushin method (the measurement method determined by the 17th Committee of the Japan Society for the Promotion of Science), specifically, the method described in "Carbon Fiber" [Otani Sugiro, pp. 733-742 (March 1986), Modern Editing Co., Ltd.].
[0105] (Average particle size)
[0106] The average particle size of the non-graphitizable carbon of the present invention is preferably 20 to 40 μm, more preferably 25 to 35 μm, because the coating film thickness can be stabilized and thickly coated for a high-capacity thick film electrode.
[0107] It should be noted that the average particle size of the non-graphitizable carbon of the present invention is the particle size (D 50 ).
[0108] (Specific surface area (BET))
[0109] In the non-graphitizable carbon of the present invention, the specific surface area (BET) obtained by the BET method based on nitrogen adsorption varies depending on the particle size and cannot be generalized. From the reason of suppressing the reactivity with the electrolyte, it is preferably 10 m 2 / g or less, more preferably 1 to 6 m 2 / g.
[0110] (True specific gravity)
[0111] The true specific gravity of the non-graphitizable carbon of the present invention is preferably 1.45 g / cm2 because the higher the true specific gravity, the higher the electrode density and the higher the volume capacity. 3 More preferably, 1.47 g / cm 3 Above, most preferably 1.49 g / cm 3 From the perspective of maintaining high discharge capacity and excellent volume capacity, the true specific gravity is preferably 1.58 g / cm 3 Below, more preferably 1.56 g / cm 3 Below, most preferably 1.54g / cm 3 the following.
[0112] In addition, the true specific gravity can be obtained by a liquid phase replacement method using a pycnometer using butanol in accordance with JIS R7222.
[0113] [Method for producing non-graphitizable carbon]
[0114] The hardly graphitizable carbon of the present invention can be obtained, for example, by the following production method. It should be noted that the production method for obtaining the hardly graphitizable carbon of the present invention is not limited to the following.
[0115] As a method for producing the non-graphitizable carbon of the present invention, for example, a method having the following steps in order is preferred because a higher discharge capacity can be obtained.
[0116] [Cross-linking treatment process]
[0117] First, a raw material of non-graphitizable carbon is subjected to a cross-linking treatment to obtain a cross-linked product.
[0118] [Infusible treatment process]
[0119] Next, the cross-linked product is subjected to an infusibility treatment to obtain an infusibility treated product.
[0120] [Pulverization process]
[0121] Next, the infusible product is subjected to a pulverization process to obtain a pulverized product.
[0122] [Firing process]
[0123] Next, the pulverized product is fired to produce non-graphitizable carbon.
[0124] Hereinafter, each step will be described.
[0125] [Cross-linking treatment process]
[0126] First, a raw material of non-graphitizable carbon (hereinafter, also simply referred to as "raw material") is subjected to a cross-linking treatment to obtain a cross-linked product.
[0127] Here, the raw material used in the method for producing carbon of the present invention can be selected to make the average interplanar spacing d002 reach the above-mentioned given range of the present invention by calcining (described later). The raw material can be selected from asphalts such as coal-based asphalt and petroleum-based asphalt; resins such as phenolic resin and furan resin; mixtures of asphalt and resin, etc., and in the case of coal-based asphalt, the average interplanar spacing d002 is easy to reach the given range, so it is preferred.
[0128] Examples of methods for crosslinking the raw materials include: a method based on an air blowing reaction; a dry method based on an oxidizing gas (air, oxygen, ozone); a wet method using an aqueous solution of nitric acid, sulfuric acid, hypochlorous acid, a mixed acid, etc. Among them, the method based on an air blowing reaction is preferred.
[0129] The air blowing reaction is a reaction in which the softening point is raised by heating the above raw materials and blowing an oxidizing gas (e.g., air, oxygen, ozone, or a mixture thereof). According to the air blowing reaction, a cross-linked product (e.g., air-blown asphalt) having a high softening point of, for example, 200° C. or higher can be obtained.
[0130] It should be noted that, according to Japanese Patent Application Laid-Open No. 9-153359, it is known that the air blowing reaction is a reaction in a liquid phase state, and compared with the cross-linking treatment in a solid phase state, oxygen atoms are basically not incorporated into the carbon material.
[0131] In the blowing reaction, an oxidative dehydration reaction is carried out as the main reaction, and polymerization is carried out through biphenyl-type cross-linking bonds. Then, through subsequent infusibility and sintering (described later), the cross-linked portion has a three-dimensional structure with no dominant orientation, and a large amount of pores for occluding lithium can be obtained.
[0132] The conditions of the air blowing reaction are not particularly limited. Since an intermediate phase is generated when the temperature is too high and the reaction rate is slowed down when the temperature is low, the reaction temperature is preferably 280 to 420°C, and more preferably 320 to 380°C. In addition, the blowing amount of the oxidizing gas is preferably 0.5 to 15 L / min per 1000 g of asphalt in terms of compressed air, and more preferably 1.0 to 10 L / min. The reaction pressure may be any of normal pressure, reduced pressure, and pressurized pressure, and is not particularly limited.
[0133] The softening point of the cross-linked product such as air-blown pitch obtained by such a cross-linking treatment is preferably 200 to 400°C, more preferably 250 to 350°C, from the perspective of ease of infusibility treatment.
[0134] The obtained cross-linked product may be coarsely pulverized using an atomizer or the like before being subjected to the infusibility treatment.
[0135] [Infusible treatment process]
[0136] Next, the above cross-linked product such as air-blown asphalt is subjected to an infusible treatment to obtain an infusible product (e.g., infusible asphalt). The infusible treatment is a cross-linking treatment (oxidation treatment) performed in a solid phase, whereby oxygen is incorporated into the structure of the cross-linked product, and further cross-linking is performed to make it difficult to melt at high temperatures.
[0137] There are no particular limitations on the method of infusibility treatment, and examples thereof include a dry method using an oxidizing gas (air, oxygen); a wet method using an aqueous solution of nitric acid, sulfuric acid, hypochlorous acid, a mixed acid, etc. Among them, a dry method using an oxidizing gas is preferred.
[0138] The treatment temperature for the infusibility treatment should be selected to be below the softening point of the cross-linked product. In order to further prevent fusion, the heating rate during batch treatment is preferably 5 to 100°C / hour, more preferably 10 to 50°C / hour.
[0139] From the viewpoint of obtaining a higher discharge capacity and making the degree of oxidation inside the particles uniform and homogenous in order to obtain stable characteristics of the non-graphitizable carbon, the number of times of the infusibility treatment is preferably divided into two or more times.
[0140] The other treatment conditions in the infusibility treatment are not particularly limited. For example, the blowing amount of the oxidizing gas is preferably 1.0 to 20 L / min, more preferably 2.0 to 10 L / min per 1000 g of compressed air. The reaction pressure may be any of normal pressure, reduced pressure, and pressurized pressure, and is not particularly limited.
[0141] The oxygen content of the infusible product obtained by the infusible treatment is preferably 3 to 20% by mass, more preferably 5 to 15% by mass, from the viewpoint of preventing fusion during firing.
[0142] [Pulverization process]
[0143] Next, the above-mentioned infusible treated product such as infusible asphalt is subjected to a pulverization treatment to obtain a pulverized treated product (infusible treated product after pulverization). By adjusting the pulverization conditions and removing unnecessary fine powder, coarse powder, and particles of special shapes in the infusible treated product after pulverization as needed, the Guinier radius Rg1 of the present invention can be controlled to a given range. It is also possible to mix two or more infusible treated products pulverized under their respective pulverization conditions to control the Guinier radius Rg1 of the present invention to a given range.
[0144] At this time, the pulverization is preferably performed so that the average particle size of the pulverized product (the infusible product after pulverization) becomes 20 to 40 μm, and more preferably 25 to 35 μm.
[0145] It should be noted that the average particle size here refers to the particle size (D 50 ).
[0146] The pulverizer used for the pulverization treatment is not particularly limited, and a conventionally known method can be used, and examples thereof include a jet mill, a pin mill, a ball mill, a hammer mill, a roll mill, and a vibration mill.
[0147] When using these pulverizers, the pulverization conditions are set so that the average particle size of the infusible product after the pulverization process falls within the above-mentioned range.
[0148] [Firing]
[0149] Next, the pulverized product is fired in an atmosphere of an inert gas such as reduced pressure or nitrogen to obtain non-graphitizable carbon. From the viewpoint of obtaining a higher discharge capacity, the temperature reached during firing (firing temperature) is preferably 600 to 900° C., more preferably 650 to 800° C. At this time, the heating rate is preferably 50 to 150° C. / hour, more preferably 80 to 120° C. / hour.
[0150] [Negative electrode for lithium-ion secondary battery]
[0151] The negative electrode for a lithium ion secondary battery of the present invention (negative electrode of the present invention) is a negative electrode for a lithium ion secondary battery containing the hardly graphitizable carbon of the present invention (carbon of the present invention).
[0152] The negative electrode of the present invention can have a high discharge capacity by containing the carbon of the present invention.
[0153] The negative electrode of the present invention is not particularly limited except that it contains the hardly graphitizable carbon of the present invention.
[0154] As a method for manufacturing the negative electrode of the present invention, for example, the following method can be cited: preparing a negative electrode mixture coating containing the non-graphitizable carbon of the present invention and a binder, and applying the above-mentioned negative electrode mixture coating to one or both surfaces of a collector to form a negative electrode mixture layer, thereby manufacturing the negative electrode of the present invention.
[0155] The binder is preferably a binder that is chemically and electrochemically stable with respect to the electrolyte. For example, polyvinylidene fluoride, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), etc. can be used as the binder.
[0156] The negative electrode mixture coating may further contain, for example, a carbon material other than the hardly graphitizable carbon of the present invention, graphite as an active material, carbon black or carbon fiber as a conductive agent, and a solvent.
[0157] The content of the hardly graphitizable carbon in the present invention is preferably about 1 to 20% by mass in the total amount of the negative electrode mixture.
[0158] The current collector used in the negative electrode of the present invention is not particularly limited. Examples of the shape of the current collector include: foil; mesh; and a mesh such as a porous metal. Examples of the material of the current collector include copper, stainless steel, and nickel.
[0159] [Lithium-ion secondary battery]
[0160] The lithium ion secondary battery of the present invention (battery of the present invention) is a lithium ion secondary battery having the negative electrode for a lithium ion secondary battery of the present invention (negative electrode of the present invention).
[0161] The battery of the present invention can have a high discharge capacity by including the negative electrode of the present invention.
[0162] The lithium ion secondary battery of the present invention is not particularly limited except that it uses the negative electrode of the present invention. The battery components other than the negative electrode may be based on the components of a general lithium ion secondary battery.
[0163] Generally, lithium-ion secondary batteries have negative electrodes, positive electrodes and non-aqueous electrolytes as their main battery components. The positive and negative electrodes are respectively formed of materials (as layered compounds) or compounds or clusters that can absorb lithium ions. The lithium ions enter and exit the layers during the charge and discharge process. It is a battery mechanism in which lithium ions are doped into the negative electrode during charging and dedoped from the negative electrode during discharge.
[0164] [negative electrode]
[0165] The negative electrode included in the lithium ion secondary battery of the present invention is not particularly limited as long as it is the negative electrode of the present invention.
[0166] [positive electrode]
[0167] As the positive electrode material (positive electrode active material), it is preferred to select a material that can be doped / dedoped with a sufficient amount of lithium ions. Examples of such positive electrode active materials include transition metal oxides, transition metal chalcogenides, vanadium oxides, and lithium-containing compounds thereof, and compounds of the general formula M X 6S 8-Y (wherein X is a value in the range of 0≤X≤4, Y is a value in the range of 0≤Y≤1, and M represents a metal such as a transition metal) represented by a Chevreul phase compound, lithium iron phosphate, activated carbon, activated carbon fiber, etc., which can be used alone or in combination of two or more. For example, carbonates such as lithium carbonate can also be added to the positive electrode.
[0168] The lithium-containing transition metal oxide is a composite oxide of lithium and a transition metal, or may be an oxide formed by solid solution of lithium and two or more transition metals. Specifically, the lithium-containing transition metal oxide is LiM(1) 1-P M(2) P O2 (wherein P is a value in the range of 0≤P≤1, and M(1) and M(2) are composed of at least one transition metal element), or LiM(1) 2-Q M(2) Q O4 (wherein Q is a value in the range of 0≤Q≤1, and M(1) and M(2) are composed of at least one transition metal element). Here, the transition metal element represented by M includes Co, Ni, Mn, Cr, Ti, V, Fe, Zn, Al, In, Sn, etc., preferably Co, Fe, Mn, Ti, Cr, V, Al.
[0169] Such lithium-containing transition metal oxides can be obtained by using, for example, Li, oxides or salts of transition metals as starting materials, mixing these starting materials according to the composition, and calcining them in an oxygen atmosphere at a temperature range of 600 to 1000° C. It should be noted that the starting materials are not limited to oxides or salts, and can also be synthesized from hydroxides and the like.
[0170] As a method for forming a positive electrode using such a positive electrode material, for example, a positive electrode mixture layer is formed by applying a paste-like positive electrode mixture coating formed by a positive electrode material, a binder and a conductive agent to one or both sides of a collector. As a binder, the binders exemplified in the negative electrode can be used. As a conductive agent, for example, particulate carbon materials, fibrous carbon materials, graphite, carbon black, VGCF (vapor grown carbon fiber) can be used. The shape of the collector is not particularly limited, and the same shape as the negative electrode can be used. As the material of the collector, aluminum, nickel, stainless steel foil, etc. can usually be used.
[0171] When forming the above-mentioned positive electrode, various additives such as conventionally known conductive agents and binders may be appropriately used.
[0172] [Electrolytes]
[0173] As the electrolyte, a common non-aqueous electrolyte containing a lithium salt such as LiPF6, LiBF4, etc. as an electrolyte salt can be used.
[0174] The non-aqueous electrolyte may be a liquid non-aqueous electrolyte solution, or may be a polymer electrolyte such as a solid electrolyte or a gel electrolyte.
[0175] In the case of a liquid nonaqueous electrolyte solution, an aprotic organic solvent such as ethylene carbonate, propylene carbonate, or dimethyl carbonate can be used as the nonaqueous solvent.
[0176] In the case of a polymer electrolyte, a matrix polymer after gelation with a plasticizer (non-aqueous electrolyte) is included. As the matrix polymer, ether polymers such as polyethylene oxide and its crosslinked products, polymethacrylates, polyacrylates, polyvinylidene fluoride, fluorine-based polymers such as vinylidene fluoride-hexafluoropropylene copolymers, etc. can be used alone or in combination, wherein, from the viewpoint of redox stability, etc., fluorine-based polymers are preferably used.
[0177] As the electrolyte salt and the non-aqueous solvent constituting the plasticizer (non-aqueous electrolyte solution) contained in the polymer electrolyte, those that can be used for liquid electrolyte solutions can be used.
[0178] In the lithium ion secondary battery of the present invention, a separator such as a microporous body of polypropylene or polyethylene or a material having a layer structure thereof or a nonwoven fabric can be generally used.
[0179] The lithium ion secondary battery of the present invention may also use a gel electrolyte. In this case, for example, the negative electrode containing the hardly graphitizable carbon of the present invention, the gel electrolyte, and the positive electrode are sequentially stacked and housed in a battery exterior material.
[0180] The structure of the lithium ion secondary battery of the present invention is arbitrary, and its shape and form are not particularly limited, and it can be arbitrarily selected from, for example, a cylindrical shape, a square shape, and a coin shape.
[0181] Example
[0182] Hereinafter, the present invention will be described in detail by giving examples, but the present invention is not limited to the examples described below.
[0183] [Difficult to graphitize carbon]
[0184] <Example 1>
[0185] 1000 g of coal-based QI-free asphalt (QI: 0.1-0.5 mass %, softening point: 82.5° C.) was placed in an autoclave equipped with an anchor-type stirring device, heated to 350° C. under a nitrogen stream, and compressed air was blown into the asphalt while flowing at 5 L / min, and heated at 350° C. for 2 hours, thereby implementing a cross-linking treatment based on an air-blowing reaction. Then, the mixture was cooled to room temperature and the contents (air-blown asphalt) were taken out.
[0186] Next, infusible asphalt was obtained by performing an infusible treatment, wherein the taken-out blown asphalt was coarsely crushed with an atomizer, placed in a rotary furnace, and the compressed air was circulated at a rate of 5 L / min while the temperature was raised at a rate of 20°C / hour, and then maintained at 200°C for 1 hour (the first infusible treatment), and then the temperature was temporarily lowered, and then raised to 250°C again and maintained for 5 hours (the second infusible treatment).
[0187] The obtained infusible pitch was pulverized using a jet mill (FS-4, manufactured by Seishin Enterprise Co., Ltd.) under conditions such that the average particle size of the pulverized product was 20 to 30 μm.
[0188] Next, 100 g of the infusible pitch subjected to the above-mentioned pulverization treatment was placed in a graphite covered container, and the temperature was raised to a calcination temperature of 850°C at a heating rate of 100°C / hour under a nitrogen flow, and calcined at 850°C for 2 hours to obtain carbon powder.
[0189] <Examples 2 to 5>
[0190] In Examples 2 to 5, carbon powders were obtained in the same manner as in Example 1 except that the calcination temperature was different from that in Example 1 (for the calcination temperature, refer to the column “calcination temperature” in Table 1).
[0191] <Comparative Example 1>
[0192] 1000 g of coal-based QI-free asphalt (QI: 0.1-0.5 mass %, softening point: 82.5° C.) was placed in an autoclave equipped with an anchor-type stirring device, heated to 350° C. under a nitrogen stream, and compressed air was blown into the asphalt while flowing at 5 L / min, and heated at 350° C. for 2 hours, thereby implementing a cross-linking treatment based on an air-blowing reaction. Then, the mixture was cooled to room temperature and the contents (air-blown asphalt) were taken out.
[0193] Next, the taken out blown asphalt was coarsely crushed with an atomizer and placed in a rotary furnace. Compressed air was circulated at 5 L / min while the temperature was raised at 20°C / hour. It was then maintained at 200°C for 1 hour. The temperature was then temporarily lowered, raised to 250°C again, and maintained at 250°C for 5 hours to implement an infusible treatment, thereby obtaining infusible asphalt.
[0194] 100 g of the obtained infusible asphalt was directly placed in a graphite covered container without being pulverized, and heated to 950°C at a heating rate of 100°C / hour under a nitrogen flow. After calcination at 950°C for 2 hours, it was pulverized under the same conditions as in Example 1 to obtain carbon powder.
[0195] <Comparative Example 2>
[0196] In Comparative Example 2, a carbon powder was obtained in the same manner as in Comparative Example 1 except that the calcination temperature was different from that in Comparative Example 1 (see the column "calcination temperature" in Table 1).
[0197] <Comparative Example 3>
[0198] In Comparative Example 3, the calcination temperature and the pulverization conditions after calcination were different from those in Comparative Example 1 (for the calcination temperature and the average particle size of the carbon powder, refer to the "calcination temperature" and "average particle size" columns in Table 1). Except for this, the carbon powder was obtained in the same manner as in Comparative Example 1.
[0199] <Comparative Example 4>
[0200] A carbon powder was obtained under the same conditions as in Comparative Example 1 except that the sintering temperature was changed to 1100° C. and the infusibility treatment was not performed.
[0201] <Comparative Example 5>
[0202] A carbon powder was obtained under the same conditions as in Comparative Example 1 except that the calcination temperature was changed to 1100° C. and ethylene bottom oil was used as a raw material.
[0203] <Comparative Example 6>
[0204] Natural graphite having an average particle size of 16 μm was used as the carbon powder.
[0205] <Evaluation of Carbon Powder>
[0206] The average particle size (unit: μm) and specific surface area (BET) (unit: m) of the carbon powders obtained in Examples 1 to 5 and Comparative Examples 1 to 6 were measured by the above-mentioned method. 2 / g), average interplanar spacing d002 of (002) plane (unit: nm), true specific gravity (unit: g / cm 3 ), Guinier radii Rg1 and Rg2 (unit: nm) obtained by small angle X-ray scattering using Guinier analysis. The above results are shown in the "Analysis Results" column of Table 1 below.
[0207] [Negative electrode, lithium-ion secondary battery]
[0208] Next, negative electrodes were prepared using the carbon powders obtained in Examples 1 to 5 and Comparative Examples 1 to 6, and evaluation batteries were prepared using the negative electrodes (see Figure 2 ), and the following evaluation was conducted.
[0209] (Preparation of negative electrode mixture paste)
[0210] First, the carbon powders obtained as described above were used as negative electrode materials to prepare negative electrode mixture paste. Specifically, carbon powder (95 parts by mass) and a 12% N-methylpyrrolidone solution of polyvinylidene fluoride (5 parts by mass in terms of solid content) were placed in a planetary mixer, stirred at 100 rpm for 15 minutes, and N-methylpyrrolidone was further added to adjust the solid content ratio to 60%, and stirring was continued for 15 minutes to prepare a negative electrode mixture paste.
[0211] (Fabrication of working electrode (negative electrode))
[0212] Each negative electrode mixture paste prepared as described above was applied to the copper foil in a uniform thickness, and then placed in a blower dryer to volatilize the solvent at 100°C to form a negative electrode mixture layer. Next, the negative electrode mixture layer was pressurized using a roller press and further punched into a circle with a diameter of 15.5 mm, thereby producing a working electrode (negative electrode) having a negative electrode mixture layer that was closely attached to the collector formed by the copper foil. It should be noted that before evaluation, drying was performed at 100°C in a vacuum for more than 8 hours.
[0213] (Preparation of Electrolyte)
[0214] In a mixed solvent of ethylene carbonate (33% by volume) and ethyl methyl carbonate (67% by volume), LiPF6 was added at a concentration of 1 mol / dm 3 The concentration of was dissolved to prepare a non-aqueous electrolyte.
[0215] (Evaluation of battery manufacturing)
[0216] Next, using each working electrode (negative electrode) prepared as described above, Figure 2 Evaluation battery shown. Figure 2 This is a cross-sectional view of an evaluation battery (coin-type secondary battery for evaluation) produced in order to evaluate battery characteristics in Examples and Comparative Examples.
[0217] For evaluation of battery production, refer to Figure 2 First, a lithium metal foil was pressed against a nickel mesh and punched into a circle with a diameter of 15.5 mm, thereby preparing a disk-shaped counter electrode (positive electrode) 4 made of lithium foil in close contact with a current collector 7a formed of the nickel mesh.
[0218] Next, the separator 5 impregnated with the electrolyte solution is sandwiched between the working electrode (negative electrode) 2 tightly attached to the collector 7b and the counter electrode 4 tightly attached to the collector 7a, and the layers are stacked. Then, the working electrode 2 is contained in the outer cup 1, the counter electrode 4 is contained in the outer can 3, the outer cup 1 and the outer can 3 are joined, and the edges of the outer cup 1 and the outer can 3 are riveted and sealed with an insulating pad 6, thereby producing an evaluation battery.
[0219] In the manufactured evaluation battery, the edges of the outer cup 1 and the outer can 3 are riveted with an insulating pad 6 interposed therebetween to form a sealed structure. Figure 2 As shown, the current collector 7a, the counter electrode 4, the separator 5, the working electrode (negative electrode) 2 and the current collector 7b are stacked in this order from the inner surface of the outer can 3 toward the inner surface of the outer cup 1.
[0220] (Charge and discharge test)
[0221] The evaluation batteries prepared as described above were subjected to the following charge and discharge tests at 25° C. In this test, the process of doping carbon powder with lithium ions is called “charge”, and the process of dedoping carbon powder is called “discharge”.
[0222] First, a constant current charge is performed at a current value of 0.39mA until the circuit voltage reaches 0mV, and then the charge is switched to a constant voltage charge when the circuit voltage reaches 0mV. Furthermore, the charge is continued until the current value reaches 20μA. The first charge capacity (unit: mAh / g) is calculated based on the amount of power supplied during this period. Then, stop for 120 minutes. Next, a constant current discharge is performed at a current value of 0.39mA until the circuit voltage reaches 1.5V, and then the discharge is switched to a constant voltage discharge when the circuit voltage reaches 1.5V. Furthermore, the discharge is continued until the current value reaches 20μA. The first discharge capacity (unit: mAh / g) is calculated based on the amount of power supplied during this period. For each evaluation battery, the results of the discharge capacity obtained are shown in the "Battery Characteristics" column of Table 1 below.
[0223] Evaluation criteria for discharge capacity
[0224] In the present invention, when the discharge capacity is 470 mAh / g or more, the discharge capacity of the non-graphitizable carbon is evaluated to be high. The larger the discharge capacity is than 470 mAh / g, the higher the discharge capacity of the non-graphitizable carbon is, and the more preferable it is.
[0225] On the other hand, when the discharge capacity is less than 470 mAh / g, it is evaluated that the discharge capacity of the non-graphitizable carbon is low.
[0226] surface
[0227]
[0228] According to the results shown in Table 1, the secondary batteries having the negative electrodes containing the carbon powders obtained in Examples 1 to 5 (corresponding to the non-graphitizable carbon of the present invention) showed high discharge capacity.
[0229] On the other hand, the discharge capacity of the secondary battery having the negative electrode containing the carbon powder obtained in Comparative Examples 1 and 2 (Rg2 was out of the given range) was low.
[0230] The discharge capacity of the secondary battery having the negative electrode containing the carbon powder obtained in Comparative Example 3 (Rg1 was out of the given range) was low.
[0231] The discharge capacity of the secondary battery having the negative electrode containing the carbon powder obtained in Comparative Example 4 (d002, Rg1, and Rg2 were outside the given ranges) was low.
[0232] The discharge capacity of the secondary battery having the negative electrode containing the carbon powder obtained in Comparative Example 5 (d002 and Rg2 were outside the given ranges) was low.
[0233] The discharge capacity of the secondary battery having the negative electrode containing the carbon powder obtained in Comparative Example 6 (d002, Rg1, and Rg2 were outside the given ranges) was low.
[0234] As described above, the hardly graphitizable carbon of the present invention has a high discharge capacity.
[0235] Furthermore, the negative electrode of the present invention containing the hardly graphitizable carbon of the present invention and the lithium ion secondary battery of the present invention having the negative electrode have high discharge capacity and are therefore useful for ESS.
Claims
1. A non-graphitizable carbon having a scattering vector q of 0.30 nm obtained by small-angle X-ray scattering measurement and Guinier analysis. -1 Above and 0.40nm -1 The following range of the Guinier radius Rg1 is 3.00 nm or more and 5.80 nm or less, The scattering vector q is 2.05nm -1 Above and 2.85nm -1 The following range of the Guinier radius Rg2 is 0.35 nm or more and 0.57 nm or less, and The non-graphitizable carbon has an average interplanar spacing d002 of (002) planes determined by X-ray diffraction of 0.365 nm or more and 0.375 nm or less. 2 . The non-graphitizable carbon according to claim 1 , which has an average particle size of 20 μm or more and 40 μm or less. 3 . The non-graphitizable carbon according to claim 1 , which has a true specific gravity of 1.45 or more and 1.58 or less. 4 . A negative electrode for a lithium ion secondary battery, comprising the hardly graphitizable carbon according to claim 1 . 5 . A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to claim 4 .
Citation Information
Patent Citations
Cylindrical complex construction for load transmission
JP1987045412B2
Carbonaceous material for secondary battery electrode
JP1995320740A
Manufacture of lithium secondary battery negative electrode material and its negative electrode material
JP1997153359A
Carbon material for anode for non-aqueous solvent secondary battery
JP1998083814A
Sodium secondary battery
WO2014157125A1