Method for preparing alkali activated cement by step-by-step calcination of sodium chloride

Through the step-by-step calcination method of sodium chloride and exhaust gas treatment, the problems of high cost and unstable performance of traditional alkali-activated cement are solved, and the preparation of alkali-activated cement with low cost, low carbon emissions and resource recovery is achieved, ensuring the stability of cement performance Reduction of sexual and pollution.

CN118084371BActive Publication Date: 2024-11-12HUNAN UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410204515.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-24
Publication Date
2024-11-12
Estimated Expiration
2044-02-24

AI Technical Summary

Technical Problem

Traditional alkali-excited cement has problems with high cost and performance instability, especially due to the scarcity of industrial alkali and kaolin resources and the high amount of alkali excitants, the production cost is high and difficult to control.

Method used

The sodium chloride step-by-step calcination method is adopted to reduce the amount of alkali exciter by mixing sodium chloride, silicate and carbonate, and the amount of alkali exciter is added to the clinker by mixing sodium hydroxide or potassium hydroxide to reduce costs. Recycle valuable metals from solid waste slag and treat exhaust gas to reduce pollution.

Benefits of technology

Low-cost preparation of alkali-activated cement is achieved, significantly reducing carbon emissions, improving resource recovery, ensuring cement performance stability, and by-production of valuable hydrochloric acid and HCl gases through exhaust gas treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004712594810000041
    Figure BDA0004712594810000041
  • Figure BDA0004712594810000051
    Figure BDA0004712594810000051
  • Figure BDA0004712594810000052
    Figure BDA0004712594810000052
Patent Text Reader

Abstract

The invention discloses a method for preparing alkali-activated cement by a sodium chloride step-by-step calcination method, wherein sodium chloride, silicate and carbonate are mixed and ground in proportion, and then calcined and rapidly cooled to obtain a calcined material, and a small amount of caustic soda is added to the calcined material and ground to obtain cement powder. The alkali-activated cement prepared by the invention has the characteristics of extensive raw materials, low cost, low consumption and low carbon emission, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of cement building materials, and particularly relates to a method for preparing alkali-activated cement by a step-by-step calcination of sodium chloride. Background Art

[0002] The preparation of silicate cement clinker has outstanding problems such as carbon emission, high energy and material consumption, serious dust and sulfur and nitrogen oxide gas pollution, and poor corrosion resistance and durability. Alkali-activated cement has outstanding advantages such as early strength, corrosion resistance and good freeze-thaw resistance. It can make use of a large amount of solid waste slag, is low-carbon, energy-saving and environmentally friendly, and is one of the new cements that is most likely to replace silicate cement. Traditional alkali-activated cement is a two-component cement hardened by using strong alkali to activate active amorphous silicate (calcium) salt. It still has many shortcomings: (1) Kaolin resources are scarce, and other main raw materials such as fly ash and blast furnace slag are used as admixtures of silicate cement in large quantities, resulting in rising prices; (2) The large amount of industrial alkali activator added (3-14wt% in terms of Na2O) also makes its cost high, and it is easy to effloresce and affect durability; (3) The inherent variability of the composition of industrial waste slag makes it difficult to stabilize and regulate the performance and preparation process of alkali-activated cement prepared with it as the main raw material.

[0003] Reducing and eliminating the use of alkali activators can effectively reduce the cost of alkali-activated cement. Patents CN110371140A and CN110451827A disclose a method for preparing and using room temperature curing and steam curing alkali-activated cement, respectively. A small amount of industrial alkali is mixed with potassium sodium aluminosilicate and calcium raw materials and ground, then calcined at 1250-1300°C and rapidly cooled to obtain clinker. The clinker is ground and evenly mixed with sodium water glass to obtain cement. The 28-day compressive strength of their cement paste exceeds 80MPa and 110MPa, respectively. The amount of alkali activator used in these two types of cement is lower than that of the commonly used two-component alkali-activated cement, but the industrial alkali and potassium sodium aluminosilicate used to calcine the clinker are not cheap, and still affect the cost of alkali-activated cement. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing alkali-activated cement by a stepwise calcination of sodium chloride, which reduces the preparation cost of alkali-activated cement by burning clinker with cheap raw materials and further reducing the amount of alkali activator.

[0005] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing alkali-activated cement by a step-by-step calcination of sodium chloride, comprising the following steps in order:

[0006] (1) mixing sodium chloride, silicate and carbonate and grinding them to a fineness that all pass through an 80-μm square-hole sieve to obtain raw material powder S1;

[0007] (2) The raw material powder S1 is first calcined at 850-1050°C, then heated to not less than 1240°C, and then rapidly cooled after calcination to obtain the clinker S2;

[0008] (3) Sodium hydroxide and / or potassium hydroxide are added to the clinker S2 and the mixture is ground into a fine powder to obtain cement powder.

[0009] As an optimization, in step (1), the mass proportion of SiO2+Al2O3+CaO+MgO in the calcined base obtained by oxidative calcination of the mixture of silicate and carbonate at 950°C is not less than 90.0%, and SiO2: 31.0-47.0%, Al2O3: 12.4-18.0%, CaO: 21.3-46.3%, MgO: 0-16.2%.

[0010] As an optimization, the amount of sodium chloride added in step (1) is 8.0 to 20.0% of the mass of the mixture of silicate and carbonate calcined at 950°C.

[0011] As an optimization, the calcination time at 850-1050° C. in step (2) is not less than 1 hour.

[0012] As an optimization, the flow rate during the calcination at 850-1050°C in step (2) is not less than 80 g min -1 ·m -2 of water vapor.

[0013] As an optimization, the calcination time at not less than 1240° C. in step (2) is not less than 1 hour.

[0014] As an optimization, the rapid cooling after the calcination in step (2) is water quenching cooling or blast cooling.

[0015] As an optimization, the mass of sodium hydroxide and / or potassium hydroxide in step (3) is calculated as (NaOH+0.713KOH) / S2=0.5-3.0%.

[0016] As an optimization, in step (3), sodium hydroxide and / or potassium hydroxide are pre-dissolved in water and mixed with the powder of clinker S2 obtained by grinding separately when the cement is used.

[0017] As an optimization, in step (2), the calcination tail gas is collected and introduced into water for dissolution, and the aqueous solution of the tail gas is subsequently treated to produce hydrochloric acid or recover valuable metals.

[0018] The beneficial effects of the present invention are:

[0019] (1) In the process of preparing cement clinker, no expensive industrial alkali is required as raw material, and the alkali used for activation is further reduced, thereby minimizing the cost of preparing alkali-activated cement.

[0020] (2) The prepared general-purpose cement uses aluminosilicate as the main raw material. Compared with silicate cement, it not only significantly reduces carbon emissions, but also can absorb a large amount of aluminosilicate solid waste.

[0021] (3) During the cement production process, valuable metals in solid waste are recovered simultaneously to improve resource recovery rate and achieve full utilization of solid waste.

[0022] (4) Heavy metals in solid waste can be removed through the chlorination roasting process, and the residual heavy metals can be solidified in cement. While achieving full utilization of solid waste containing heavy metals, the risk of heavy metal pollution is eliminated through "double insurance".

[0023] (5) The tail gas discharged during the cement production process can be used to produce HCl gas and hydrochloric acid. DETAILED DESCRIPTION

[0024] The present invention is further described in detail by specific examples, but the scope of the present invention is not limited thereto. The steps of raw material powder preparation, raw material calcination, cement preparation and curing, and calcination tail gas solution treatment are described as follows.

[0025] 1. Raw material powder preparation

[0026] The silicates with the main chemical composition of SiO2 and Al2O3 used in this application include granite, kaolin, quartz sandstone and lithium tailings, carbonates include limestone and dolomite, and lead-zinc tailings are a mixture of silicates and carbonates. Among them, the lead-zinc tailings contain a small amount of lead and zinc sulfides. All embodiments are quantitatively mixed with the above-mentioned silicates and carbonates or their mixtures (see Table 1) to obtain a calcium-magnesium-aluminosilicate mixture. The mixture is sampled and ground and oxidized and calcined at 950°C to obtain a calcined base. The ingredients of the calcium-magnesium-aluminosilicate mixture must make the mass proportion of SiO2+Al2O3+CaO+MgO in its calcined base not less than 90.0%, and SiO2: 31.0-47.0%, Al2O3: 12.4-18.0%, CaO: 21.3-46.3%, MgO: 0-16.2%. The amount of sodium chloride added is 8.0-20.0% of the calcined mass of the calcium-magnesium-silicate-aluminate mixture, and the sodium chloride and the calcium-magnesium-silicate-aluminate mixture are mixed together to obtain raw meal. The raw meal is ground to a fineness that can completely pass through an 80-micron square hole sieve to obtain raw meal powder S1.

[0027] 2. Raw material calcination

[0028] The raw material powder S1 is loaded into a boat-shaped corundum crucible and placed in the corundum vacuum tube of the silicon carbide tubular atmosphere furnace. The outlet of the atmosphere furnace is equipped with an acid-resistant quartz flange, and the inlet is connected to the air or water vapor atmosphere as needed. The vent pipe at the outlet is connected to water. The tubular furnace is heated to 500℃ at a rate of 5℃ / min, and the atmosphere is connected. The air atmosphere only needs to keep the gas in the tube moving in one direction, and the flow rate of water vapor must be no less than 80g·min -1 ·m -2 , when the working temperature rises to 850-1050°C, keep the temperature constant for 1.0-4.0 hours. After the constant temperature is over, continue to heat up to 1240°C or higher at a rate of 5°C / min and keep the temperature constant for 1-3 hours. After the calcination is over, stop the water vapor input, quickly remove the quartz flange at the gas outlet, take the crucible out of the tube while it is hot, and cool the clinker S2 in the crucible by blasting (air cooling) or water quenching (water cooling). The main chemical composition of the calcined base of the calcium magnesium silicate mixture, the amount of sodium chloride and the calcination system in each embodiment are shown in Table 2.

[0029] 3. Cement preparation and maintenance

[0030] Grind S2 into powder with cement fineness, dissolve NaOH and / or KOH with as little water as possible and cool to room temperature, and the added mass of NaOH and / or KOH is determined according to (NaOH+0.713KOH) / S2=0.5-3.0. Mix the alkaline solution with the clinker powder and stir for 2-5 minutes. Add water quantitatively during stirring to reduce the consistency of the slurry so that the slurry can be liquefied during subsequent vibration. Move the slurry into a 40×40×40 steel mold and vibrate it to compact it. Then move it together with the mold into a cement standard curing box and curing it at 20℃ and ≧90% humidity for 1 day before demoulding. When the strength in 1 day does not meet the demoulding requirements, delay demoulding, and then continue standard curing in moisture for 3 days, 7 days and 28 days, and test the compressive strength of test blocks of different ages. See Table 3 for details of cement slurry ingredients and compressive strength. It can be seen from Table 3 that with the increase of alkali content, the strength of cement shows an increasing trend, and the maximum compressive strength of cement paste after 28 days reaches 82.5MPa.

[0031] 4. Treatment of calcination tail gas solution

[0032] The chemical composition of the cooled clinker S2 was detected. The residual Cl ion content in the roasted slag ranged from 0.08% to 1.35% (see Table 3 for details). Most of them were close to the chlorine content (0.10%) required for general silicate cement. By increasing the final calcination time, the chlorine content can be reduced to the cement standard requirement (see Example 12). The lead and zinc content in Example No. 2 was much lower than that in the lead-zinc tailings, with a Pb removal rate of 90.5% and a Zn removal rate of 66.4%. The lead and zinc metal removed in this example was dissolved in the water connected to the tail gas and can be recovered by physical and chemical treatment. The tail gas solution of other examples that do not contain valuable metals and heavy metals can be distilled to obtain purified HCl gas, which can be dissolved in water to obtain hydrochloric acid.

[0033] Table 1 Proportion of silicate and carbonate raw materials in raw materials of each embodiment Unit: %

[0034]

[0035] Table 2 Main chemical composition, sodium chloride content and calcination system of calcium magnesium silicate raw material calcination base in raw meal

[0036]

[0037] a Unit: g·min -1 ·m -2

[0038] Table 3 List of chlorine content of cement clinker, cement paste ingredients and compressive strength

[0039]

Claims

1. A method for preparing alkali activated cement by stepwise calcination of sodium chloride, characterized in that: The steps include the following sequence: (1) Sodium chloride, silicate and carbonate are mixed and ground to a fineness that all of them pass through an 80-μm square-hole sieve to obtain raw material powder S1, wherein the mass proportion of SiO2+Al2O3+CaO+MgO in the calcined base obtained by oxidative calcination of the mixture of silicate and carbonate at 950°C is not less than 90.0%, and SiO2: 31.0-47.0%, Al2O3: 12.4-18.0%, CaO: 21.3-46.3%, MgO: 0-16.2%, and the amount of sodium chloride added is 8.0-20.0% of the mass of the calcined base of the mixture of silicate and carbonate at 950°C; (2) The raw material powder S1 is first calcined at 850-1050°C, then heated to not less than 1240°C, and then rapidly cooled after calcination to obtain the clinker S2; (3) The clinker S2 is mixed with one or both of sodium hydroxide and potassium hydroxide, and ground into cement powder. The mass of sodium hydroxide and / or potassium hydroxide added is calculated as (NaOH+0.713KOH) / S2=0.5-3.0%.

2. The method for preparing alkali activated cement by the stepwise calcination of sodium chloride as claimed in claim 1, characterized in that: The calcination time at 850-1050° C. in step (2) is not less than 1 hour.

3. The method for preparing alkali activated cement by the stepwise calcination of sodium chloride as claimed in claim 1, characterized in that: During the calcination at 850-1050°C in step (2), the flow rate is not less than 80 g / min -1 ·m -2 of water vapor.

4. The method for preparing alkali activated cement by the stepwise calcination of sodium chloride as claimed in claim 1, characterized in that: The calcination time at a temperature not lower than 1240° C. in step (2) is not less than 1 hour.

5. The method for preparing alkali activated cement by the stepwise calcination of sodium chloride as claimed in claim 1, characterized in that: After the calcination in step (2) is completed, water quenching or blast cooling is performed.

6. The method for preparing alkali activated cement by the stepwise calcination of sodium chloride as claimed in claim 1, characterized in that: In step (3), sodium hydroxide and / or potassium hydroxide are pre-dissolved in water and mixed with the powder obtained by grinding the clinker S2 separately when the cement is used.

7. The method for preparing alkali activated cement by the stepwise calcination of sodium chloride as claimed in claim 1 or 5, characterized in that: In the step (2), the calcination tail gas is collected and introduced into water for dissolution, and the aqueous solution of the tail gas is subsequently treated to produce hydrochloric acid or recover valuable metals.