A high-activity, long-life self-supporting hydrogen evolution electrode and preparation method thereof

By using two-electrode electroplating method on a nickel-based metal support to form porous metal phosphides and coat them with dense nickel layer, the problem of active substances falling off during the alkaline electrolysis of water hydrogen production is solved, and high activity and Long-life alkaline electrolytic water electrode.

CN118086947BActive Publication Date: 2024-12-06CRINM (GUANGDONG) INST FOR ADVANCED MATERIALS & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410443214.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-12-06
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

The active substances of existing transition metal phosphides are prone to fall off and dissolve during the process of alkaline electrolysis of hydrogen production, resulting in difficulty in maintaining activity and stability, especially in high current density, long-life electrodes are difficult to achieve.

Method used

The two-electrode electroplating method is used to grow metal phosphides on the nickel-based metal support, and a porous structure is formed through high current, and then a dense nickel coating is formed at low current to improve the self-support strength and stability of the electrode and prevent alkaline erosion.

Benefits of technology

It significantly improves the activity and stability of the electrode in alkaline electrolysis of water hydrogen, ensuring high activity and stability of the electrode during long-term electrolysis, especially under high current density, the electrode life exceeds 500 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118086947B_ABST
    Figure CN118086947B_ABST
Patent Text Reader

Abstract

The invention discloses a high-activity, long-life self-supporting hydrogen evolution electrode and a preparation method thereof, which belongs to the field of hydrogen evolution material preparation, and the method steps include: using a nickel-based metal carrier as a cathode, placing the electrode in a first electroplating solution, applying a first current, and electroplating for a first time; placing the electrode in a second electroplating solution, applying a second current, and electroplating for a second time, and then performing a cyclic voltammetry scan; the first electroplating solution contains hypophosphite and a metal salt, the second electroplating solution contains a nickel salt and ammonium sulfite, the first current is greater than the second current, and the first time is greater than the second time. This method can greatly improve the activity of the electrode in the production of hydrogen by alkaline electrolysis of water, the metal phosphide is coated with metal nickel to effectively isolate the alkali solution from corroding the active metal phosphide, and ensure the stability of the electrode during long-term electrolysis, the obtained electrode coating is tightly connected to the nickel-based metal carrier, and there are a large number of pores, which are conducive to the escape of the product, and effectively ensure the activity and stability of hydrogen production under high current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a high-activity, long-life self-supporting hydrogen evolution electrode and a preparation method thereof, belonging to the technical field of hydrogen evolution material preparation. Background Art

[0002] Excessive consumption of fossil fuels can lead to serious environmental pollution and energy crisis. Therefore, there is an urgent need to develop clean, renewable and low-carbon technologies to upgrade the existing energy structure. Hydrogen (H2) is a green and clean energy with the characteristics of light weight, high calorific value and pollution-free combustion. It is considered to be an ideal choice for solving environmental pollution and fossil energy depletion problems. It is expected to play an important role in power generation systems, transportation, industrial energy, and residential cogeneration in the future. At present, there are three main methods for industrial hydrogen production: methane steam reforming, coal gasification and water electrolysis. Methane reforming and coal gasification are suitable for large-scale production of hydrogen. However, they are heavily dependent on fossil fuels and do not meet the requirements of reducing carbon emissions. In addition, they produce a large amount of carbon dioxide and carbon monoxide byproducts, which can easily cause downstream catalyst poisoning. In contrast, water electrolysis has the advantages of high hydrogen purity, zero carbon emissions and environmental friendliness, and is the most promising hydrogen production method. Among them, alkaline water electrolysis hydrogen production equipment has mature technology, low manufacturing and maintenance costs, large single-tank hydrogen production scale, and is suitable for large-scale hydrogen demand in industries such as petrochemicals. It has been established as the water electrolysis hydrogen production technology closest to large-scale industrial realization.

[0003] However, the catalyst Raney nickel currently used in industrial alkaline water electrolysis for hydrogen production has good stability but low activity. Therefore, in recent years, researchers have developed many materials and strategies to improve the activity and stability of catalysts. For example, transition metal chalcogenides, transition metal nitrides, transition metal carbides, transition metal phosphides, metal alloy materials, etc. all show excellent alkaline water electrolysis activity. Among them, transition metal phosphides are considered to be one of the most promising transition metal-based alkaline water electrolysis hydrogen production catalysts. However, the performance of transition metal phosphides is not stable enough under alkaline conditions, and there is a problem of easy detachment of the catalyst during the electrolysis process, which makes it impossible to maintain activity and stability. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the present invention provides a high-activity, long-life self-supporting hydrogen evolution electrode and a preparation method thereof, which can avoid the shedding and dissolution of active substances of transition metal phosphides during alkaline water electrolysis, and at the same time have high activity and stability.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] In a first aspect, the present application provides a method for preparing a high-activity and long-life self-supporting hydrogen evolution electrode, comprising the following steps: using a two-electrode electroplating method, using a nickel-based metal carrier as a cathode, placing the electrode in a first electroplating solution, applying a first current, and electroplating for a first time; then placing the electrode in a second electroplating solution, first applying a second current, electroplating for a second time, and then performing a cyclic voltammetry scan, removing the cathode, and obtaining the high-activity and long-life self-supporting hydrogen evolution electrode;

[0007] The first electroplating solution contains 10g / L~50g / L hypophosphite and 5g / L~80g / L metal salt; the second electroplating solution contains 10g / L~100g / L nickel salt and 1g / L~15g / L ammonium sulfite; the first current is greater than the second current, and the first time is greater than the second time.

[0008] The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode provided in the present application grows a metal phosphide on a nickel-based metal carrier, which can improve the activity of the electrode in hydrogen production by alkaline electrolysis of water, and electroplating with a plating solution with higher plating activity and a higher current to form a relatively loose and porous metal phosphide, which can greatly improve the hydrogen production activity of the electrode, and then electroplating with a plating solution with lower plating activity and a lower current to form a dense metal nickel-coated metal phosphide as a protective layer, which improves the self-supporting strength of the electrode to a certain extent and isolates the metal phosphide from the corrosion of the alkaline solution, so that the electrode has both high hydrogen production activity and long-term stability.

[0009] Furthermore, the nickel-based metal carrier includes nickel foam, nickel mesh or nickel fiber felt.

[0010] Furthermore, the nickel-based metal carrier is pretreated, and the pretreatment step includes: placing the nickel-based metal carrier in an alkaline solution for ultrasonic cleaning, then washing with water until neutral, then placing it in an acid solution for ultrasonic cleaning, and finally washing with water until neutral.

[0011] Alkaline washing can remove oil stains on the surface of the nickel-based metal support, and acid washing can remove oxides on the surface of the nickel-based metal support, which can improve the adhesion of the subsequent metal phosphide growth on the metal support and prevent the metal phosphide from falling off during the electrolytic hydrogen evolution process.

[0012] Furthermore, the alkali solution includes 1g / L~2g / L NaOH, 5g / L~9g / L Na2CO3, and 8g / L~14g / L Na3PO4, and the nickel-based metal carrier is ultrasonically cleaned in the alkali solution for more than 30 minutes.

[0013] Sodium hydroxide is the main component for washing oil stains, and sodium carbonate and sodium phosphate are used to improve the surface tension of the alkali solution, which can promote the washing effect.

[0014] Furthermore, the acid solution is 1M~3M HCl, H2SO4 or HNO3, and the time for ultrasonic cleaning of the nickel-based metal carrier in the acid solution is 10min~20min.

[0015] Furthermore, the metal salt in the first electroplating solution includes at least one of nickel salt, cobalt salt, copper salt, divalent iron salt, and molybdate; the first current is -500mA / cm 2 , the first time is 15 minutes.

[0016] Under this current, nickel, cobalt, copper, iron, and molybdenum can be reduced and loose metal phosphides can be formed.

[0017] Furthermore, the metal salt in the first electroplating solution is selected from at least one of NiSO4·6H2O, Ni(NO3)2·6H2O, CoSO4·7H2O, Co(NO3)2·6H2O, NaMoO4·2H2O, FeSO4·7H2O, and CuSO4·5H2O, and halogen-containing metal salts are not used to avoid changes in the electrode surface morphology.

[0018] Furthermore, the second current is -50 mA / cm 2 The second time is 3 minutes, the voltage range of the cyclic voltammetry scan is -1.3V~-2.8V, the scanning speed is 20mV / s, and a total of 10 scans are performed, so that the nickel coating and the metal phosphide can be more closely combined, the self-supporting strength of the electrode is improved, the compactness of the nickel coating is improved, and the protective effect on the metal phosphide is enhanced.

[0019] Furthermore, the first electroplating solution also contains 10 g / L to 50 g / L of boric acid and 60 g / L to 150 g / L of sodium citrate.

[0020] In a second aspect, the present application also provides a high-activity and long-life self-supporting hydrogen evolution electrode, which is made by the high-activity and long-life self-supporting hydrogen evolution electrode preparation method described in the first aspect and has both high activity and stability.

[0021] The beneficial effects of the present invention are as follows: the present invention grows metal phosphides on a nickel-based metal carrier, which greatly improves the activity of the electrode in producing hydrogen by alkaline electrolysis of water; a layer of metal nickel is coated on the outer layer of the metal phosphide to effectively isolate the alkali solution from corroding the active metal phosphide, thereby ensuring the stability of the electrode during long-term electrolysis; the obtained electrode coating is tightly connected to the nickel-based metal carrier, and a large number of pores exist, which is conducive to the escape of the product, thereby effectively ensuring the hydrogen production activity and stability under high current density.

[0022] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope image of NiCoMoP-NM in Example 1 of the present application.

[0024] Figure 2 This is a comparison chart of the electrochemical performance of the electrodes prepared in Examples 1, 2, and 3 of the present application and a commercial nickel mesh.

[0025] Figure 3 = -200 mA / cm of NiCoMoP-NM in Example 1 of this application 2 Constant current stability test results.

[0026] Figure 4 = -1000 mA / cm of NiCoMoP-NM in Example 1 of this application 2 Constant current stability test results. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings of the embodiments of the present disclosure. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] It should be understood that, under the premise of no conflict, any and all embodiments of the present invention can be combined with the technical features in any other embodiment or multiple other embodiments to obtain another embodiment. The present invention includes such a combination to obtain another embodiment.

[0029] Unless otherwise specified, all technical and scientific terms used herein have the standard meanings in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.

[0030] The catalytic activity of transition metal phosphides under alkaline conditions needs to be further improved, and the activity and stability are difficult to maintain for a long time. In current research, the focus is mainly on improving the catalytic activity of transition metal phosphides, and less attention is paid to the stability of the materials, especially at high current density (≥ 100 mA / cm 2) There are still few reports on electrodes with long life (>500 h). It is urgent to avoid the shedding and dissolution of active substances and prepare alkaline water electrolysis electrodes with both high activity and stability.

[0031] In view of the above-mentioned deficiencies in the prior art, in order to solve the problem that catalytic activity and stability cannot be taken into account at the same time, the embodiment of the present application provides a method for preparing a high-activity and long-life self-supporting hydrogen evolution electrode, comprising the following steps:

[0032] A two-electrode electroplating method is adopted, with a nickel-based metal carrier as the cathode, the electrode (including the anode and the cathode) is placed in a first electroplating solution, a first current is applied, and the electroplating is performed for a first time; then the electrode is placed in a second electroplating solution, a second current is first applied, the electroplating is performed for a second time, and then a cyclic voltammetry scan is performed, and the cathode is removed to obtain a high-activity and long-life self-supporting hydrogen evolution electrode.

[0033] The first electroplating solution contains 10g / L~50g / L hypophosphite and 5g / L~80g / L metal salt; the second electroplating solution contains 10g / L~100g / L nickel salt and 1g / L~15g / L ammonium sulfite; the first current is greater than the second current, and the first time is greater than the second time.

[0034] The anode during electroplating can be made of nickel, graphite, platinum and other materials, which are conductive and do not introduce other impurities. The cathode after electroplating is the target product, and the growth of metal phosphide on the nickel-based metal carrier can improve the activity of the electrode in the production of hydrogen by alkaline electrolysis of water.

[0035] In the first round of electroplating, a plating solution with high electroplating activity and a large current are used. Under a large current, water decomposition accompanies the electroplating process, and the gas produced by hydrolysis continuously overflows from the coating, thereby creating many gaps in the coating and forming a porous metal phosphide with a large surface area, which can greatly improve the hydrogen production activity of the electrode. Preferably, the first current is -500mA / cm 2 , the first time is 15min. Each molecule of hypophosphite is reduced to obtain one electron, and it is easy to control the phosphorus content in the metal phosphide by controlling the amount of metal salt and hypophosphite.

[0036] In the second round of electroplating, a plating solution with lower electroplating activity and a smaller current are used to form a dense metal nickel-coated metal phosphide. Preferably, the second current is -50 mA / cm 2, the second time is 3min, the voltage range of cyclic voltammetry scanning is -1.3V~-2.8V, the scanning speed is 20mV / s, and a total of 10 scans. Ammonium sulfite can promote the deposition of nickel on metal phosphide, making the nickel coating more compact, and ammonium sulfite plays a certain corrosion inhibition role, reducing the presence of oxide impurities in the coating and improving the quality of the nickel coating. As a protective layer, the nickel coating improves the self-supporting strength of the electrode to a certain extent, and isolates the alkali solution from the corrosion of the metal phosphide, so that the electrode has both high hydrogen production activity and long-term stability.

[0037] The nickel-based metal carrier used for the cathode includes nickel foam, nickel mesh or nickel fiber felt, which has a large surface area and is beneficial to further improve the catalytic activity of the finished product.

[0038] Preferably, the nickel-based metal carrier is pretreated, and the pretreatment step includes: placing the nickel-based metal carrier in an alkali solution for ultrasonic cleaning to remove oil, then washing with water until neutral, then placing it in an acid solution for ultrasonic cleaning to remove surface oxides, and finally washing with water until neutral. Wherein, the alkali solution includes 1g / L~2 g / L of NaOH, 5g / L~9 g / L of Na2CO3, 8g / L~14g / L of Na3PO4, and the time for ultrasonic cleaning of the nickel-based metal carrier in the alkali solution is more than 30 minutes. The acid solution is 1M~3M HCl, H2SO4 or HNO3, and the time for ultrasonic cleaning of the nickel-based metal carrier in the acid solution is 10min~20min.

[0039] The metal salt in the first electroplating solution is selected from at least one of NiSO4·6H2O, Ni(NO3)2·6H2O, CoSO4·7H2O, Co(NO3)2·6H2O, NaMoO4·2H2O, FeSO4·7H2O, and CuSO4·5H2O. The first electroplating solution also contains 10 g / L to 50 g / L of boric acid and 60 g / L to 150 g / L of sodium citrate. Example 1

[0040] Cut the nickel mesh (NM) into 1cm*2cm pieces and put it into alkaline solution, which is a mixture of 1.5 g / L NaOH, 7 g / L Na2CO3 and 10 g / L Na3PO4. Ultrasonicate in the alkaline solution for 30 min, then wash with water until neutral. Put the nickel mesh into 1 M HCl and continue ultrasonicating for 15 min. After completion, wash with water until neutral, and put it into exhausted analytical grade ethanol for storage.

[0041] The pretreated nickel mesh was placed in the first electroplating solution, which was dissolved by 20 g / L NiSO4·6H2O, 5 g / L CoSO4·7H2O, 5 g / L NaMoO4·2H2O, 25 g / L NaH2PO2·H2O, 30 g / L H3BO3, and 100 g / L sodium citrate. A two-electrode system was used for electroplating. The treated nickel mesh was connected to the negative electrode of the power supply as the cathode during electroplating, and the commercial untreated nickel mesh was connected to the positive electrode of the power supply as the anode during electroplating. A 1cm*1cm portion of the cathode nickel mesh was immersed in the electroplating solution at -500 mA / cm 2 The current density was set to -50 mA / cm2 for 15 min, followed by washing away the surface plating solution with water. The surface was then placed in a second plating solution consisting of 20 g / L NiSO4·6H2O and 4 g / L (NH4)2SO3 dissolved therein. 2 The electroplating was carried out for 3 min at a current density of -1.3V~-2.8V, followed by cyclic voltammetry scanning at a scanning speed of 20 mV / s for 10 cycles. The surface electroplating solution was washed off with water, and the cathode was removed to obtain the electrode NiCoMoP-NM. The coating was observed under an electron microscope. Figure 1 As shown, the coating is uniform and there are a lot of pores on the surface, which is conducive to the overflow of H2 produced by electrolysis of water. Example 2

[0042] Cut the nickel mesh into 1cm*2cm pieces and put it into alkaline solution, which is a mixture of 1.5 g / L NaOH, 7 g / L Na2CO3 and 10 g / L Na3PO4. Ultrasonicate in the alkaline solution for 30 minutes and then wash with water until neutral. Put the nickel mesh into 1 M HCl and continue ultrasonicating for 15 minutes. After completion, wash with water until neutral and put it into exhausted analytical grade ethanol for storage.

[0043] The pretreated nickel mesh was placed in the first electroplating solution, which was prepared by dissolving 25 g / L Ni(NO3)2·6H2O, 10 g / L NaMoO4·2H2O, 24 g / L NaH2PO2·H2O, 22 g / L H3BO3, and 100 g / L sodium citrate. A two-electrode system was used for electroplating. The treated nickel mesh was connected to the negative electrode of the power supply as the cathode during electroplating, and the commercial untreated nickel mesh was connected to the positive electrode of the power supply as the anode during electroplating. A 1cm*1cm portion of the cathode nickel mesh was immersed in the electroplating solution at -500 mA / cm 2 The current density was set to -50 mA / cm2 for 15 min, followed by washing away the surface plating solution with water. The sample was then placed in a second plating solution consisting of 20 g / L NiSO4·6H2O and 4 g / L (NH4)2SO3 dissolved in water. 2The electroplating was performed for 3 min at a current density of 1.504 nm, followed by cyclic voltammetry scanning in the voltage range of -1.3 V to -2.8 V at a scanning speed of 20 mV / s for 10 cycles. The surface electroplating solution was washed away with water to obtain the electrode NiMoP-NM. Example 3

[0044] Cut the nickel foam (NF) into 1cm*2cm pieces and put it into alkaline solution, which is a mixture of 1.5 g / L NaOH, 7 g / L Na2CO3 and 10 g / L Na3PO4. Ultrasonicate for 30 min in the alkaline solution and then wash with water until neutral. Put the nickel mesh into 1 M HCl and continue ultrasonicating for 15 min. After completion, wash with water until neutral and put it into exhausted analytical grade ethanol for storage.

[0045] The pretreated nickel foam was placed in the first electroplating solution, which was dissolved by 30 g / L Ni(NO3)2·6H2O, 25 g / L NaH2PO2·H2O, 30 g / L H3BO3, and 100 g / L sodium citrate. A two-electrode system was used for electroplating. The treated nickel mesh was connected to the negative pole of the power supply as the cathode during electroplating, and the commercial untreated nickel mesh was connected to the positive pole of the power supply as the anode during electroplating. A 1cm*1cm portion of the cathode nickel mesh was immersed in the electroplating solution at -500 mA / cm 2 The current density was set to -50 mA / cm2 for 15 min, followed by washing away the surface plating solution with water. The surface was then placed in a second plating solution consisting of 20 g / L NiSO4·6H2O and 4 g / L (NH4)2SO3 dissolved therein. 2 The electroplating was performed for 3 min at a current density of -1.3 V to -2.8 V, followed by cyclic voltammetry scanning at a scanning speed of 20 mV / s for 10 cycles. The surface electroplating solution was washed away with water to obtain the electrode NiP-NF.

[0046] Electrochemical tests were performed on the electrodes prepared in Example 1, Example 2 and Example 3. Specifically, a 1 cm*1 cm portion of the prepared electrode with deposited active material was cut off as a working electrode, Hg / HgO was used as a reference electrode, and a Pt sheet was used as a counter electrode. A linear sweep voltammetry test was performed in a 30% KOH electrolyte at room temperature with a sweep rate of 5 mV / s and an iR compensation of 90%. The test results are shown in FIG. Figure 2 The electrode prepared in Example 1 was also tested for constant current stability, with current intensities of -200 mA / cm 2 and -1000 mA / cm 2 , the results are as follows Figure 3 and Figure 4As shown. The results show that the electrodes prepared in Example 1, Example 2 and Example 3 all exhibit excellent alkaline water electrolysis hydrogen production activity, far exceeding the activity of commercial nickel mesh under the same conditions. The embodiments of the present application greatly improve the stability of the original metal phosphide, and the electrode stability is greater than 500 h. It is proved that the electrode prepared by this method has high catalytic activity, long life and universal applicability. The method of the embodiments of the present application is simple to operate, low in cost, easy to scale up and prepare, and can be prepared on a large scale in an electroplating plant.

[0047] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0048] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A method for preparing a high-activity and long-life self-supporting hydrogen evolution electrode, characterized in that: The following steps are involved: A two-electrode electroplating method is adopted, with a nickel-based metal carrier as a cathode, the electrode is placed in a first electroplating solution, a first current is applied, and electroplating is performed for a first time; then the electrode is placed in a second electroplating solution, a second current is first applied, electroplating is performed for a second time, and then a cyclic voltammetry scan is performed, and the cathode is removed to obtain the high-activity and long-life self-supporting hydrogen evolution electrode; The first electroplating solution contains 10g / L~50g / L hypophosphite and 5g / L~80g / L metal salt, and the metal salt includes at least one of nickel salt, cobalt salt, copper salt, divalent iron salt, and molybdate; the second electroplating solution contains 10g / L~100g / L nickel salt and 1g / L~15g / L ammonium sulfite; the first current is greater than the second current, and the first time is greater than the second time.

2. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 1, characterized in that: The nickel-based metal carrier includes nickel foam, nickel mesh or nickel fiber felt.

3. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 1, characterized in that: The nickel-based metal carrier is pretreated, and the pretreatment steps include: placing the nickel-based metal carrier in an alkali solution for ultrasonic cleaning, then washing with water until neutral, then placing it in an acid solution for ultrasonic cleaning, and finally washing with water until neutral.

4. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 3, characterized in that: The alkali solution includes 1g / L~2g / L NaOH, 5g / L~9g / L Na2CO3, and 8g / L~14g / L Na3PO4, and the nickel-based metal carrier is ultrasonically cleaned in the alkali solution for more than 30 minutes.

5. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 3, characterized in that: The acid solution is 1M to 3M HCl, H2SO4 or HNO3, and the time for ultrasonic cleaning of the nickel-based metal carrier in the acid solution is 10min to 20min.

6. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 1, characterized in that: The first current is -500mA / cm 2 , the first time is 15 minutes.

7. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 6, characterized in that: The metal salt in the first electroplating solution is selected from at least one of NiSO4·6H2O, Ni(NO3)2·6H2O, CoSO4·7H2O, Co(NO3)2·6H2O, NaMoO4·2H2O, FeSO4·7H2O, and CuSO4·5H2O.

8. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 1 or 6, characterized in that: The second current is -50 mA / cm 2 The second time is 3 minutes, the voltage range of the cyclic voltammetry scan is -1.3V~-2.8V, the scanning speed is 20mV / s, and a total of 10 scans are performed.

9. The method for preparing a high-activity, long-life self-supporting hydrogen evolution electrode according to claim 1 or 6, characterized in that: The first electroplating solution also contains 10 g / L to 50 g / L of boric acid and 60 g / L to 150 g / L of sodium citrate.

10. A highly active and long-life self-supporting hydrogen evolution electrode, characterized in that: The method for preparing a high-activity and long-life self-supporting hydrogen evolution electrode is described in any one of claims 1 to 9.