A polyurethane rigid foam material, preparation method and system
By using contactless pressurization technology in the production of polyurethane hard bubbles, the circular bubbles are converted into flat pressure bubbles, which solves the complex and high cost of the production process of polyurethane hard bubbles, and achieves lower thermal conductivity and Higher production efficiency.
Patent Information
- Application Number
- CN202410343757.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-03-25
AI Technical Summary
The production process of polyurethane hard foam materials is complex, has high cost, and is difficult to further reduce its thermal conductivity. Traditional methods have problems such as high equipment requirements, many production steps, limited size and uneven performance.
The liquid mixture is subjected to non-contact pressurization in the pressure chamber to form a flat pressure bubble. Combined with physical methods and chemical technology, the thermal conductivity is reduced, the production steps are simplified and the cost is reduced.
It realizes efficient and convenient preparation of polyurethane hard foam materials, reduces production costs, and improves the consistency of thermal conductivity and production efficiency of the materials.
Smart Images

Figure CN118108976B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polyurethane rigid foam materials, and in particular relates to a polyurethane rigid foam material, a preparation method and a system. Background Art
[0002] Polyurethane rigid foam is a kind of rigid foam plastic made by the reaction of polyol and isocyanate. It belongs to the polyurethane family and can be made into rigid foam, soft foam or elastomer according to its chemical structure and manufacturing process. Polyurethane rigid foam has high density, stable structure, good thermal insulation, chemical resistance and mechanical strength. Polyurethane rigid foam is widely used in many fields, such as construction industry, refrigeration and air conditioning, packaging materials, automotive industry, etc.
[0003] The main characteristics of polyurethane rigid foam materials include: extremely low thermal conductivity makes it an excellent thermal insulation material; it has high compressive strength and flexural strength; it can resist erosion by a variety of chemicals and has good moisture resistance; although it is light in weight, it has good structural strength and stability; with the advancement of technology, new polyurethane rigid foam materials pay more and more attention to environmental protection and strive to reduce the impact on the environment.
[0004] Polyurethane rigid foam has become one of the indispensable materials in modern industry and daily life due to its excellent performance and wide application. With the development of materials science, its production process and application range will continue to expand, especially in terms of environmental protection and sustainability.
[0005] In recent years, polyurethane rigid foam has made great breakthroughs in reducing foam density and thermal conductivity due to the introduction of new process methods such as low boiling point foaming agents and black and white material prepolymerization. According to the thermal conductivity formula λ=λ g +λ s +λ r , where λ g is the thermal conductivity of the gas in the pores, λ s is the thermal conductivity of the network structure, λ r is the thermal conductivity of radiation. In daily research on reducing thermal conductivity, λ is mainly targeted g That is, to reduce the thermal conductivity of the gas as much as possible. This includes the thermal conductivity of the pore gas itself, increasing the number of bubbles, reducing the bubble diameter, etc. When λ is at 0.016w / mk, it is very difficult to further reduce the thermal conductivity, which is close to the limit.
[0006] Based on this problem, conventional methods generally use chemical and physical methods to achieve it, for example, by improving the raw materials, but this method has little effect on the thermal insulation due to the nature of the material itself; for another example, there is an existing method for preparing materials using vacuum insulation panel technology, which includes mixing the raw materials with a foaming agent, then compressing the mixed material downward using a physical high-pressure plate, cutting and heat-treating the material after compression, and finally sealing the material and vacuuming the preparation method. Although this method can make the material obtain a lower thermal conductivity and thus obtain a high-performance insulation effect, it has potential defects or limitations, including:
[0007] (1) Complex production process: The entire production process involves multiple steps, each of which requires precise control of conditions such as temperature, pressure, and time. This increases the complexity and cost of production.
[0008] (2) High equipment requirements: In order to achieve high-pressure compression and ensure the uniformity of the material, special equipment is required, such as high-pressure foaming machines, high-pressure compression equipment, vacuum equipment, heat treatment equipment, and cutting equipment. The purchase and maintenance costs of these equipment are high.
[0009] (3) Size limitation: This method requires a specific mold and a specific pressing plate corresponding to the mold to physically press the material in the mold. The material formed by mold compression may be limited by the size of the mold, which may affect the production efficiency and material utilization of large-size products.
[0010] (4) Consistency of physical properties: The compression process is a physical process of direct downward pressure. Due to the amount of material, the fluidity, hardness, brittleness, toughness of the material, the distribution of the material in the mold, the contact area between the pressing plate and the material, and the uniformity of the pressure of the pressing plate on the material surface, uneven density and bubble distribution may occur inside the material, which may affect the physical properties and consistency of the final product.
[0011] (5) The influence of heat treatment and film sealing process on performance: The heat treatment process needs to be precisely controlled to avoid degradation of material performance. Since the intermediate product needs to be sealed in the film sealing material and the pressure is reduced to 0.1 to 0.01 Torr to achieve vacuum, this low-pressure condition has high requirements for the film sealing material. Therefore, the film sealing vacuum step needs to ensure the sealing performance. Any leakage on the surface of the film sealing material will significantly affect the insulation performance of the finished product.
[0012] Although polyurethane rigid foam has become an indispensable material for modern industry and daily life due to its excellent insulation performance and wide application, its production process and performance optimization still face major challenges. In traditional technologies, raw material issues and harsh production and manufacturing conditions, such as equipment, specific contact pressurization methods, heat treatment at specific temperatures, and vacuum treatment to avoid leakage after film sealing, can improve the performance of polyurethane rigid foam to a certain extent, but greatly increase production costs. These inherent defects and challenges have stimulated the exploration of more efficient and convenient production methods with lower production costs and higher benefits, as well as the need for further optimization of material properties. Summary of the invention
[0013] In order to solve the above problems, the present invention provides a method for preparing a polyurethane rigid foam material, comprising:
[0014] A liquid mixture is obtained according to the polyurethane raw material;
[0015] pouring the liquid mixture into a mold cavity of a curing mold for reaction;
[0016] The curing mold is placed in a pressure chamber and pressurized so that the liquid mixture fills the mold cavity of the curing mold under absolute pressure and the round bubbles in the liquid mixture form flat pressure bubbles, and the polyurethane rigid foam material is obtained after curing.
[0017] Preferably, the bubble density of the round bubbles generated in the liquid mixture is 500 / cm 3 -1000pcs / cm 3 ;
[0018] Preferably, the diameter of the round bubbles is 10 μm-20 μm.
[0019] Preferably, the polyurethane raw material comprises: a reaction composition, an isocyanate substance and a foaming agent;
[0020] The reaction composition includes water, nanocellulose, ionic liquid, perfluoroolefin, organotin and organobismuth catalysts;
[0021] Preferably, the reaction composition comprises the following components in parts by weight:
[0022] Water 1-8;
[0023] Nanocellulose 0.05-2.5;
[0024] Ionic liquid 0.1-3.5;
[0025] Perfluoroolefins 0.5-2.5;
[0026] Organic tin 0.1-0.6;
[0027] Organic bismuth catalyst 0.1-0.5;
[0028] Preferably, the reaction composition further comprises the following components:
[0029] Polyester polyols, polyether polyols, silicone oils and amine catalysts;
[0030] Preferably, the amine catalyst is selected from any one of cyclohexylamine, bis(2-dimethylaminoethyl) ether, triethylamine and N,N-dimethylbenzylamine;
[0031] Preferably, the reaction composition further comprises the following components in parts by weight:
[0032] Polyester polyol 10-30;
[0033] Polyether polyol 45-89;
[0034] Silicone oil 1-4;
[0035] Amine catalysts 1-4;
[0036] Preferably, the blowing agent is selected from any one or more of pentane, neopentane, methyl formate, HFC-245fa, LBA, R600, R600a, R-152a, R-134a, R-1234yf, opteon 1100 / 1150, HCFO-1224yd, HCFO-1234ze, HCFO-1243zf, and HCFO-1233xf.
[0037] Preferably, the liquid mixture is prepared according to the polyurethane raw material, comprising:
[0038] Taking each component in the reaction composition and mixing it to prepare the reaction composition;
[0039] Dividing the foaming agent into two parts, namely a first foaming agent and a second foaming agent;
[0040] The isocyanate substance and the first blowing agent are mixed to obtain a first mixture; the reaction composition and the second blowing agent are mixed to obtain a second mixture; wherein the ratio of the first mixture to the second mixture is: first mixture: second mixture = (1.0-1.8): (0.8-1.6); and, in the first mixture, based on the total amount being 100%, the isocyanate substance accounts for 70%-100%; the first blowing agent is the balance; in the second mixture, based on the total amount being 100%, the reaction composition accounts for 70%-100%; the second blowing agent is the balance;
[0041] The first mixed material and the second mixed material are mixed to obtain the liquid mixed material.
[0042] Preferably, placing the curing mold into a pressure chamber and pressurizing the pressure chamber comprises:
[0043] Detecting and obtaining the milky time and gel time corresponding to the liquid mixture;
[0044] Determining the time condition for pressurization in the pressure chamber according to the milky time and the gel time;
[0045] Based on the time condition, the pressure vessel is pressurized.
[0046] Preferably, the time conditions include reaction standing time and pressurization duration;
[0047] The reaction standing time is the time during which the liquid mixture is poured into the curing mold and allowed to stand for reaction; and when the reaction standing time ends, the standing is ended at the end time point and pressurization is started;
[0048] The pressurization duration is the duration of starting pressurization and maintaining the pressurized state after the liquid mixture is poured into the curing mold and the reaction standing time is over.
[0049] Preferably, the reaction standing time is calculated as follows:
[0050] T 反应 =T 乳白 ×N;
[0051] Among them, T 反应 T is the reaction standing time; 乳白 is the milky time; N is the first calculation coefficient, and its value range is 1.2-1.5.
[0052] Preferably, the calculation method of the boost duration is:
[0053] T 结束 =T 凝胶 ×M;
[0054] Among them, T 结束 is the boost duration; T 凝胶 is the gel time; M is the second calculation coefficient, and its value range is 0.8-1.6.
[0055] Preferably, the external boost pressure when pressurizing the pressure chamber is an absolute pressure;
[0056] The pressure value of the external boost pressure is between 0.5 bar and 1.5 bar.
[0057] Preferably, when the pressure chamber is pressurized, the pressure direction of the external boosting pressure applied by the boosting device is any angle within the range of 45°-135° relative to the upper surface of the liquid mixture in the curing mold.
[0058] Preferably, when pressurizing the pressure chamber, the method further comprises vibrating the mold where the curing mold is located;
[0059] Preferably, the vibration frequency of the vibration treatment is 20 Hz-20000 Hz.
[0060] In addition, in order to solve the above problems, the present invention also provides a polyurethane rigid foam material, which is prepared by the preparation method of the polyurethane rigid foam material as described above;
[0061] Preferably, the bubbles in the polyurethane rigid foam material are flat pressure bubbles, and their shape is an elongated ellipse; the vertical height of the flat pressure bubble is smaller than the horizontal length;
[0062] Preferably, the diameter of the vertical cross section of the flat pressure bubble is not greater than 3000 nm;
[0063] Preferably, the diameter d of the vertical cross section of the flat pressure bubble meets the following conditions:
[0064] 70nm<d≤3000nm.
[0065] In addition, in order to solve the above problems, the present invention also provides a system for preparing a polyurethane rigid foam material, which is prepared based on the method for preparing a polyurethane rigid foam material as described above;
[0066] The preparation system of the polyurethane rigid foam material comprises:
[0067] Pressure chambers, curing moulds and pressurising equipment;
[0068] The curing mold is provided with a mold cavity for placing the liquid mixture for preparing the polyurethane rigid foam material;
[0069] The curing mold can be placed in the pressure chamber;
[0070] The pressurizing device is connected to the pressure chamber and can increase the pressure in the pressure chamber;
[0071] Preferably, the preparation system of the polyurethane rigid foam material further comprises a vibration device connected to the curing mold;
[0072] Preferably, the preparation system of the polyurethane rigid foam material further comprises a pressurization angle adjustment device disposed on the top of the pressure chamber;
[0073] The boost angle adjustment device comprises a fixed base arranged on the top of the pressure chamber, an adjustment part connected to the fixed base and placed in the pressure chamber, and a pressure interface arranged on the upper end of the fixed base;
[0074] The pressure interface is connected to the boosting device via a pipeline;
[0075] The adjustment part includes a horizontal rotation axis, an angle adjustment axis and an output port which are connected in sequence.
[0076] The present invention provides a method for preparing a polyurethane rigid foam material, comprising: preparing a liquid mixture according to a polyurethane raw material; pouring the liquid mixture into a mold cavity of a curing mold for reaction; placing the curing mold in a pressure bin, and pressurizing the pressure bin so that the liquid mixture fills the mold cavity of the curing mold under absolute pressure, and the round bubbles in the liquid mixture form flat pressure bubbles, and the polyurethane rigid foam material is obtained after curing. The method for preparing a polyurethane rigid foam material provided by the present invention combines physical methods with chemical technologies, and non-contact pressurization is performed on the prepared liquid mixture in a pressure bin so that the liquid mixture fills the curing mold under absolute pressure, and the round bubbles in the liquid mixture form flat pressure bubbles, and the polyurethane rigid foam material is obtained after curing, which can significantly reduce λg, λs, and λr, respectively, thereby obtaining a lower thermal conductivity, and the preparation conditions and production environment are simple, the production consumables are few, the method steps are simple, and the production cost is greatly reduced, which provides a more efficient and convenient, lower production cost, and higher efficiency production method and approach for the preparation of polyurethane rigid foam materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] Figure 1 A schematic diagram of the structure and connection relationship of the method for preparing the polyurethane rigid foam material of the present invention;
[0078] Figure 2 It is a schematic diagram of the conversion of round bubbles into flat pressure bubbles during the pressurization of the liquid mixture in the method for preparing the polyurethane rigid foam material of the present invention;
[0079] Figure 3 A schematic diagram of the morphology of a flat pressure bubble in the method for preparing a polyurethane rigid foam material of the present invention;
[0080] Figure 4 A schematic diagram of the structure and connection relationship of the preparation system of the polyurethane rigid foam material of the present invention;
[0081] Figure 5 A schematic diagram of the connection relationship of the central control device of the preparation system of the polyurethane rigid foam material of the present invention;
[0082] Figure 6 The central control device of the preparation system of the polyurethane rigid foam material of the present invention compares the different pressure directions investigated in Experiment 3.
[0083] Reference numerals:
[0084] 100, preparation system of polyurethane rigid foam material; 1, pressure chamber; 2, curing mold; 21, mold cavity; 3, boosting device; 31, boosting motor; 4, vibration device; 41, vibration motor; 5, boosting angle adjustment device; 51, fixed base; 52, adjustment part; 521, horizontal rotating shaft; 5211, rotating motor; 522, angle adjustment shaft; 5221, angle adjustment motor; 523, output port; 53, pressure interface; 6, central control device; 61, bus; 62, processor; 63, storage module; 64, input module; 65, output module; 66, power supply module; 200, liquid mixture; 201, round bubble; 202, flat pressure bubble.
[0085] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0086] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0087] refer to Figure 1 The present invention provides a method for preparing a polyurethane rigid foam material, comprising:
[0088] Step S1, preparing a liquid mixture according to polyurethane raw materials;
[0089] Step S2, pouring the liquid mixture into a mold cavity of a curing mold for reaction;
[0090] Step S3, placing the curing mold into a pressure chamber and pressurizing the pressure chamber so that the liquid mixture fills the mold cavity of the curing mold under absolute pressure, and the round bubbles in the liquid mixture form flat pressure bubbles, and the polyurethane rigid foam material is obtained after curing.
[0091] For further reference, Figure 2 and Figure 3 The bubble density of the round bubbles generated in the liquid mixture is 500 / cm 3 -1000pcs / cm 3 ;
[0092] Furthermore, the diameter of the round bubbles is 10 μm-20 μm.
[0093] The round bubbles are generated by the reaction of the liquid mixture after mixing, and their diameter d 圆形气泡 The range is 10μm-20μm.
[0094] As mentioned above, the curing mold can be any desired shape of the finished polyurethane rigid foam material. Since the liquid mixture is a liquid or semi-fluid, it is placed in the mold cavity of the curing mold and can "fill" the entire cavity according to the shape of the mold cavity of the curing mold, and in the further pressurization process, the liquid mixture can further spread the mold cavity (spread and fill the space in the mold cavity at the corresponding height according to the amount of liquid mixture added), making the shape more uniform, more fitting and consistent with the mold cavity of the curing mold.
[0095] As mentioned above, the curing mold can be placed in a pressure chamber, and the pressure chamber can be an independent chamber body, or a chamber body composed of an upper cover connected to the curing mold.
[0096] In the field of materials science and engineering, especially in the preparation of polymer foams, the technology of applying pressure by directly contacting the material with a physical press plate is usually called "physical compression method" or "direct compression method". This method involves the use of physical force (such as through a press plate) to directly act on the material to change its density, shape or structure. It is often used in the processing of foam materials such as polyurethane rigid foam to achieve specific physical properties.
[0097] In the present invention, the method of applying pressure to the material in a space with positive pressure (pressure chamber) without physical contact can be classified as "non-contact pressure application method" or "gas pressure method". This technology relies on the gas pressure (such as air or other gas) in a closed space to apply uniform pressure on the material, thereby affecting its foaming, density or other related physical properties.
[0098] Compared with the conventional method, the method adopted by the present invention has the following specific differences and effects:
[0099] 1. Physical compression method:
[0100] (1) Although high pressure can be applied to the material in a relatively short period of time, directly affecting the density and structure of the material and quickly forming a product of a specific shape or density, it is extremely easy to cause uneven compression of the material, especially for samples with uneven mixing and uneven concentration, resulting in inconsistent toughness, hardness, and concentration of different parts of the material. Especially for products with irregular shapes, the compressed material may show different densities and properties in different areas;
[0101] (2) Secondly, the physical compression method relies on the pressure plate to directly apply pressure to the material. It may be difficult to ensure that the material completely fills the space of the mold, especially for complex shapes or small parts. If the initial placement of the material is uneven or the downward pressure of the pressure plate is not completely aligned with the mold opening, the material may not reach every corner of the mold.
[0102] (3) Due to direct physical contact compression, the uniformity of material distribution in the mold is affected by the pressing speed and force of the pressing plate and the fluidity of the material itself, which may cause the material to have high density in some areas of the mold and low density in other areas, affecting the quality and performance of the final product.
[0103] 2. Gas pressure method:
[0104] (1) The gas pressure method used in the present invention has a more uniform pressure than conventional techniques, and is suitable for the overall material to be prepared in the present invention. The product produced has a higher consistency in properties.
[0105] (2) The gas pressure method compresses the material by applying gas pressure in a closed space. This method can apply pressure to the material more evenly and is particularly suitable for applications with complex shapes or where high material density consistency is required. The gas pressure can act more evenly on each surface of the material, helping the material to quickly and evenly fill the mold cavity.
[0106] (3) Since the gas pressure method is non-contact, it can avoid the problem of uneven compression or material damage caused by direct contact between the pressing plate and the material. This method is more suitable for applications in the present invention that require higher surface quality or structural integrity of the material.
[0107] As mentioned above, after the liquid mixture reacts inside the material, a large number of round bubbles will be generated, and then when a positive pressure is applied to the space where the liquid mixture is located based on the gas pressure method, the round bubbles inside the liquid mixture will form specific, elliptical and long bubbles, which are flat pressure bubbles.
[0108] It should be noted that in recent years, polyurethane rigid foam has made significant breakthroughs in reducing foam density and thermal conductivity due to the introduction of new process methods such as low-boiling point foaming agents and black and white material prepolymerization. g +λ s +λ r , where λ g is the thermal conductivity of the gas in the pores, λ sis the thermal conductivity of the network structure, and λr is the thermal conductivity of radiation. In the daily scientific research on reducing thermal conductivity, λg is mainly targeted, that is, the thermal conductivity of the gas is reduced as much as possible. This includes the thermal conductivity of the pore gas itself, increasing the number of bubbles, reducing the bubble diameter, etc. When λ is at 0.016w / mk, it is very difficult to further reduce the thermal conductivity, which is close to the limit.
[0109] In order to achieve the above effect, in the present invention, a gas pressure method is used to apply positive pressure to the material, so that the original round bubble is transformed into a long elliptical flat pressure bubble extending in the horizontal direction, thereby reducing the diameter of the original bubble. The principle is to control the material at λ s Infinite path effect is introduced, that is, the solid path extends the grid skeleton to infinitely extend the heat conduction path, heat is difficult to conduct at the gas-solid interface, and infinite pores make the heat transfer path infinitely long, so that the transferred heat tends to the minimum limit; and, at λ g In terms of heat dissipation, the "zero convection" effect is introduced to minimize the diameter of the bubble, and the original round bubble is flattened into a flat ellipse by external pressure to make its narrowest diameter as close to the nanometer level 70nm as possible, forming the Knudsen effect. Since the narrowest diameter in the bubble is reduced, the free movement of gas particles is restricted, the thermal convection of gas molecules in the bubble is eliminated, the effective collision of gas molecules is reduced, and the heat transfer rate is reduced; while in λ r Infinite heat baffle effect is introduced, that is, infinite hole walls are equivalent to heat shields, which reduces the heat of thermal radiation to a minimum and makes heat transfer more effective; that is, the method provided in the present invention can produce infinite path effect, zero convection effect and heat baffle effect, while reducing λ g , s and λ r .
[0110] The preparation method of the polyurethane rigid foam material provided by the present invention combines physical methods with chemical technologies, and non-contact pressurization is performed on the prepared liquid mixture in the pressure chamber, so that the liquid mixture fills the curing mold under absolute pressure, and the round bubbles in the liquid mixture are formed into flat pressure bubbles, and the polyurethane rigid foam material is obtained after curing, which can make λ g , s and λ r The preparation conditions and production environment are simple, the production consumables are few, the method steps are simple, the production cost is greatly reduced, and a more efficient, convenient, lower production cost and higher benefit production method and approach are provided for the preparation of polyurethane rigid foam materials.
[0111] Furthermore, the polyurethane raw material includes: a reaction composition, an isocyanate substance and a foaming agent;
[0112] The reaction composition comprises water, nanocellulose, ionic liquid, perfluoroolefin, organic tin and organic bismuth catalysts.
[0113] The perfluoroolefin mentioned above may be, for example, perfluoro-4-methyl-2-pentene.
[0114] As mentioned above, the isocyanate substance may be isocyanate, for example, BASF M20S.
[0115] As mentioned above, nanocellulose is a nanoscale material extracted from plant fibers, which has high strength, high specific surface area and good chemical stability. Adding nanocellulose to polyurethane foam can be used as a physical enhancer to improve the mechanical strength and toughness of the foam. In addition, the high specific surface area of nanocellulose can effectively stabilize the foam structure, reduce the pore diameter, and make the foam more uniform and delicate, thereby improving its thermal insulation performance and sound absorption capacity.
[0116] As mentioned above, ionic liquids are a type of liquid salt composed of ions, which is liquid at room temperature and has very low vapor pressure and good thermal stability. For example, it can be 1-butyl-3-methylimidazolium hexafluorophosphate.
[0117] Introducing ionic liquids in the preparation process of polyurethane foam can act as a reaction medium or catalyst to affect the reaction kinetics of polyols and isocyanates. Ionic liquids can adjust the rate and direction of polymerization reactions, help control the growth and stability of foams, and achieve a finer and more uniform pore structure. In addition, ionic liquids may also affect the cell opening and closing properties of foams, further optimizing their performance.
[0118] As mentioned above, perfluoroolefin is a fluorinated hydrocarbon compound with extremely low surface energy and excellent chemical inertness. When added to polyurethane foam, this perfluoroolefin can be used as a physical foaming agent, and the gas foam formed during the polymerization process helps to reduce the cell diameter and increase the number of cells. The addition of perfluoroolefin can also improve the water repellency and chemical stability of the foam, thereby extending its service life.
[0119] The principle of adding these three materials, nanocellulose, ionic liquid and perfluoroolefin, is mainly based on their unique physical and chemical properties. They work together in the preparation process of polyurethane foam through physical enhancement (nanocellulose), chemical regulation (ionic liquid) and physical foaming (perfluoroolefin). This composite effect helps to achieve a smaller and more uniform pore structure, improve the thermal insulation, mechanical properties and chemical stability of the foam, and meet the high requirements for the performance of polyurethane foam materials in specific application areas. In this way, the structure and properties of polyurethane foam can be optimized, and its performance can be precisely controlled. The pore diameter can be effectively reduced to 10μm-20μm, while the number of bubbles can be increased to 500 / cm 3 -1000pcs / cm3 .
[0120] The organic tin (for example, DABCO-7120) and organic bismuth catalyst (for example, BiCAT 8124) can control the time distance between the milky time and the gel time, and at the same time improve the activation period, the toughness and ductility of the cell wall.
[0121] In addition, it should be noted that perfluoroolefins and organic bismuth catalysts have a certain synergistic effect. In the preparation process of polyurethane rigid foam, the combination of specific raw materials and their interaction have an important influence on the properties of the final product. The synergistic effect of perfluoroolefins and organic bismuth catalysts can be analyzed from the perspective of chemistry and physics. The details are as follows:
[0122] (1) Chemical perspective:
[0123] Perfluoroolefins act as nucleating agents, promoting the production of bubbles during the polymerization reaction and affecting the cell structure of the foam. They may also react with isocyanates to form a stable bubble interface, which helps maintain the stability of the foam.
[0124] Bismuth-based catalysts (such as BiCAT 8124) are highly effective catalysts that accelerate the reaction between isocyanates and polyols, thereby promoting polymerization. Bismuth-based catalysts are particularly effective in catalyzing the three-component (isocyanate, polyol, water) reaction, which is critical to the formation of polyurethane foam.
[0125] The formation of polyurethane mainly involves the following chemical reactions:
[0126] NCO + HO-R-OH → NH-CO-OR-OH;
[0127] Among them, NCO represents an isocyanate group and HO-R-OH represents a polyol.
[0128] Perfluoroolefin acts as a nucleating agent to promote the formation of bubbles. Organic bismuth acts as a catalyst to accelerate the above reaction, but is not consumed in the reaction.
[0129] (2) Physical perspective:
[0130] In the process of forming polyurethane foam, perfluoroolefins act as nucleating agents to reduce the surface tension of the mixture and promote the formation and growth of bubbles, which helps control the pore size and distribution of the foam. Organobismuth catalysts accelerate chemical reactions and reduce the time required for polymerization, thereby affecting the milky time (the time it takes for the mixture to transform from a liquid to a milky solid) and the gel time (the time it takes for the mixture to fully solidify). Accelerating the reaction also helps to form a stable foam structure in a shorter time, thereby improving the toughness and ductility of the bubble wall.
[0131] The synergistic effect between perfluoroolefins and organobismuth catalysts is mainly reflected in their joint promotion of the formation of polyurethane rigid foam and optimization of the foam's microstructure and macroscopic properties. This synergistic effect helps to achieve a more uniform and stable foam structure, improves the foam's mechanical properties, such as toughness and ductility, and also achieves energy conservation and consumption reduction in the preparation process.
[0132] Furthermore, the reaction composition includes the following components in parts by weight:
[0133] Water 1-8;
[0134] Nanocellulose 0.05-2.5;
[0135] Ionic liquid 0.1-3.5;
[0136] Perfluoroolefins 0.5-2.5;
[0137] Organic tin 0.1-0.6;
[0138] Organic bismuth catalyst 0.1-0.5;
[0139] Furthermore, the reaction composition further includes the following components:
[0140] Polyester polyols, polyether polyols, silicone oils and amine catalysts;
[0141] Furthermore, the reaction composition further includes the following components in parts by weight:
[0142] Polyester polyol 10-30;
[0143] Polyether polyol 45-89;
[0144] Silicone oil 1-4;
[0145] Amine catalysts 1-4;
[0146] Further, the amine catalyst is selected from any one of cyclohexylamine, bis(2-dimethylaminoethyl) ether, triethylamine and N,N-dimethylbenzylamine;
[0147] Furthermore, the blowing agent is selected from any one or more of pentane, neopentane, methyl formate, HFC-245fa, LBA, R600, R600a, R-152a, R-134a, R-1234yf, opteon 1100 / 1150, HCFO-1224yd, HCFO-1234ze, HCFO-1243zf, and HCFO-1233xf.
[0148] As mentioned above, foaming agents can be divided into the following categories:
[0149] (1) Hydrocarbons
[0150] Pentane: An alkane compound used as a physical blowing agent.
[0151] Neopentane: It belongs to hydrocarbon substances and is also a physical foaming agent. It can form bubbles in the material during processing, thereby reducing weight, increasing volume, and improving heat insulation, sound insulation and other properties.
[0152] R600 and R600a: refer to n-pentane and isopentane respectively, both of which are physical foaming agents with low GWP.
[0153] (2) Hydrofluorocarbons (HFCs)
[0154] HFC-245fa: A hydrofluorocarbon used as a blowing agent with low ozone depletion potential (ODP) and medium GWP.
[0155] R-152a: Another hydrofluorocarbon with a low GWP value, used to replace traditional high GWP HFCs blowing agents.
[0156] R-134a: An HFC compound widely used in coolants and also as a blowing agent, but due to its high GWP, it is gradually being replaced by low-GWP alternatives.
[0157] (3) Low Global Warming Potential (Low GWP) Gases
[0158] R-1234yf, HCFO-1224yd, HCFO-1234ze, HCFO-1243zf, HCFO-1233xf: These are low GWP gases belonging to the group of hydrofluoroolefins (HFOs) and hydrochlorofluoroolefins (HCFOs). They are developed as less environmentally friendly alternatives to traditional HFCs blowing agents with high global warming potential.
[0159] LBA: Solstice LBA (HFO-1233zd, 1-chloro-3,3,3-trifluoropropene) is a chemical belonging to the hydrofluoroolefin (HFO) class of blowing agents, designed specifically for the production of polyurethane foams.
[0160] (4) Others
[0161] Methyl formate: An organic compound used as a blowing agent, especially in the production of bio-based or environmentally friendly polyurethane foams.
[0162] Opteon 1100 / 1150: This is a series of low GWP blowing agents produced by Chemours, mainly based on HFO and other formulations, used to provide excellent thermal insulation performance and reduce environmental impact.
[0163] The choice of each blowing agent depends on the specific application of the desired foam material, the performance requirements, and environmental impact considerations. The use of low GWP blowing agents is gaining more and more attention to reduce greenhouse gas emissions and the impact of global warming.
[0164] Furthermore, the step S1, preparing a liquid mixture according to the polyurethane raw material, comprises:
[0165] Step S11, mixing the components in the reaction composition to prepare the reaction composition;
[0166] Step S12, dividing the foaming agent into two parts, namely a first foaming agent and a second foaming agent;
[0167] Step S13, mixing the isocyanate substance and the first blowing agent to obtain a first mixture; mixing the reaction composition with the second blowing agent to obtain a second mixture; wherein the ratio of the first mixture to the second mixture is:
[0168] First mixture: second mixture = (1.0-1.8): (0.8-1.6);
[0169] Furthermore, in the first mixed material, the isocyanate substance accounts for 70%-100% of the total amount; the first foaming agent is the balance;
[0170] In the second mixed material, the reaction composition accounts for 70%-100% of the total amount; the second foaming agent is the balance;
[0171] Step S14: mixing the first mixed material and the second mixed material to obtain the liquid mixed material.
[0172] As mentioned above, in step S14, the first mixed material and the second mixed material are mixed, and the mixing may be stirred, so as to prepare a liquid mixed material.
[0173] Furthermore, the step S3, placing the curing mold in a pressure chamber and pressurizing the pressure chamber, includes:
[0174] Step S31, detecting and obtaining the milky time and gel time corresponding to the liquid mixture;
[0175] Step S32, determining a time condition for pressurization in the pressure chamber according to the milky time and the gel time;
[0176] Step S33, pressurizing the pressure chamber based on the time condition.
[0177] As mentioned above, the detection of cream time and gel time can be performed separately by using a small sample of the prepared liquid mixture. Cream time and gel time are two important reaction time parameters in the production process of polyurethane foam, which respectively indicate the time points when the material starts to foam and the material starts to solidify. These two parameters are crucial to controlling the quality and performance of polyurethane foam. For example, the following is a basic method for detecting these two time parameters:
[0178] (1) Cream Time Detection
[0179] Preparation: Prepare the polyol and isocyanate components according to the product formulation.
[0180] Mixing: Mix the polyol and isocyanate together under appropriate conditions (usually room temperature), using a mechanical stirrer to ensure thorough mixing.
[0181] Observation: Start timing immediately after mixing and observe the color change of the mixture. Cream time is the time from the start of mixing to the time when the mixture begins to turn milky white (i.e., begins to foam). This time point is usually determined by visual observation.
[0182] (2) Gel Time Detection
[0183] Continue to observe: After determining the milky time, continue to observe the changes in the state of the mixture.
[0184] Test: Test the mixture by periodically tapping it with a suitable tool (such as a metal or glass rod) to test for changes in viscosity and structure.
[0185] Note: Gel time is the time from the beginning of mixing to the time when the mixture loses fluidity and begins to solidify. This is usually determined by observing the time when the mixture changes from a flowing state to a solid or semi-solid state (no flow and keeps shape).
[0186] It should be noted that environmental conditions (such as temperature and humidity) have a significant impact on milky time and gel time, so the test should be consistent with the environmental conditions used in formal production. Use an accurate timer to record the time to ensure the accuracy of the results. For different formulations and applications, the ideal values of milky time and gel time may be different, so it is necessary to ensure that the tested materials are consistent with the materials used in formal production.
[0187] In short, the accurate determination of milk time and gel time is of great significance for optimizing the production process of polyurethane foam and ensuring product performance. By precisely controlling these parameters, it can be ensured that the polyurethane foam has the ideal physical and chemical properties to meet the needs of specific applications.
[0188] Furthermore, the time condition in step S32 includes reaction standing time and pressurization duration;
[0189] The reaction standing time is the time during which the liquid mixture is poured into the curing mold and allowed to stand for reaction; and when the reaction standing time ends, the standing is ended at the end time point and pressurization is started;
[0190] The pressurization duration is the duration of starting pressurization and maintaining the pressurized state after the liquid mixture is poured into the curing mold and the reaction standing time is over.
[0191] As mentioned above, the reaction standing time includes the time control of two operating behaviors:
[0192] (1) The time for the liquid mixture to be poured into the curing mold for reaction;
[0193] (2) When the reaction standing time ends, the standing time is terminated and pressurization is started;
[0194] That is, the reaction standing time, that is, the standing time of the liquid mixture reaction. At the same time, the time point when the reaction standing time ends is the start time point of pressurization.
[0195] After the boosting device is started to start boosting, boosting is continued according to the boosting duration, and boosting is stopped at the end of the time period.
[0196] For example, if the reaction standing time = 8 seconds and the pressurization duration = 51 seconds, the following process can be used:
[0197] (1) 15:00:00-15:00:08, after pouring the liquid mixture into the mold cavity of the curing mold, let it stand for 8 seconds to react;
[0198] (2) 15:00:08, the pressure chamber began to be pressurized, which lasted for 51 seconds;
[0199] (3) 15:00:59, the 51-second countdown ends and the pressurization stops.
[0200] Further, the calculation method of the reaction standing time is:
[0201] T 反应 =T 乳白 ×N;
[0202] Among them, T 反应 T is the reaction standing time; 乳白is the milky time; N is the first calculation coefficient, and its value range is 1.2-1.5. For example, N can be 1.2, 1.3, 1.4, 1.5, etc.
[0203] Furthermore, the calculation method of the boost duration is:
[0204] T 结束 =T 凝胶 ×M;
[0205] Among them, T 结束 is the boost duration; T 凝胶 is the gel time; M is the second calculation coefficient, and its value range is 0.8-1.6. For example, M can be 0.9, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, etc.
[0206] In the above, N and M are the calculation coefficients corresponding to the reaction static time and the pressurization duration, respectively. It is proved by experiments that under a certain positive pressure, the T calculated by the corresponding calculation coefficient is 反应 and T 结束 The prepared polyurethane rigid foam material can achieve better effects under the premise of controlling the preparation time.
[0207] Furthermore, the external boost pressure when the pressure chamber is pressurized is an absolute pressure;
[0208] The pressure value of the external boost pressure is between 0.5 bar and 1.5 bar, for example, 0.6 bar, 0.7 bar, 0.8 bar, 0.9 bar, 1.0 bar, 1.1 bar, 1.2 bar, 1.3 bar, 1.4 bar, 1.5 bar, etc.
[0209] Furthermore, when the pressure chamber is pressurized, the pressure direction of the external boosting pressure applied by the boosting device is any angle within the range of 45°-135° relative to the upper surface of the liquid mixture in the curing mold.
[0210] For example, it may be 45°, 50°, 55°, 60°, 65°, 70°, 75°, 80°, 85°, 90°, 95°, 100°, 105°, 110°, 115°, 120°, 125°, 130°, 135°, and so on.
[0211] The direction in which pressure is applied has a significant effect on the morphology of polyurethane rigid foam, especially the size, shape and distribution of bubbles (pores). This is because the formation of polyurethane rigid foam involves a chemical reaction after the raw materials are mixed, including the reaction of the isocyanate component with the polyol component, and the evaporation of the blowing agent or the chemical generation of gases, which form the bubbles in the foam structure. The application of pressure can change the growth and stability of the bubbles in the mixture, which in turn affects the physical properties of the final rigid foam, such as thermal conductivity, strength and density.
[0212] The effect of applied pressure on the morphology of rigid foam is as follows:
[0213] (1) Bubble nucleation and growth: The applied pressure can affect the formation and growth rate of bubble nuclei. Higher pressure tends to reduce the size of bubbles because it increases the solubility of gas inside the bubbles, thereby delaying the formation and growth of bubbles.
[0214] (2) Bubble shape control: If the applied pressure is directional (e.g., applying greater pressure in a specific direction), it can promote the extension of the bubble in the specific direction, forming a non-spherical bubble, such as an elliptical or long strip. This effect is due to the different bubble growth rates caused by the pressure difference in different directions. Moreover, the effect is particularly obvious when the short-time gas pressure method in the present invention is used to apply pressure.
[0215] (3) Bubble distribution uniformity: The applied pressure can also affect the uniformity of bubble distribution in the rigid foam material. Uniformly applied pressure helps to form a more uniform bubble distribution, while uneven pressure may lead to uneven bubble distribution.
[0216] (4) Direction of pressure application to form bubbles of a specific shape:
[0217] To form a stack of bubbles of a certain size in the horizontal direction that are long elliptical strips, the ideal pressure application direction should be perpendicular to the direction in which the bubbles need to extend. In other words, if the bubbles need to extend horizontally to form long strips, the pressure should be applied perpendicular to the horizontal direction, which can promote the stretching and extension of the bubbles in the horizontal direction while limiting their growth in the vertical direction.
[0218] (5) Scope of pressure application:
[0219] The pressure applied needs to be high enough to ensure extension of the bubble in the desired direction, but not so high as to crush the bubble or excessively inhibit its growth.
[0220] The specific value of the pressure will depend on many factors, including the specific composition of the raw materials, the type of blowing agent and the reaction conditions. Usually, this needs to be optimized through experiments to achieve the best bubble morphology and physical properties.
[0221] For example, applying pressure downward at a 90° angle: This means that the pressure is applied perpendicular to the surface of the liquid mixture. This approach usually promotes relatively uniform growth of bubbles in all directions, because the pressure is applied perpendicular to the surface of the mixture, which has a more uniform effect on the direction of bubble growth. If there are no other forces (such as flow or gravity) affecting the directional growth of bubbles, this may not lead to the formation of long, oval bubbles.
[0222] Another example is applying pressure at an angle of 45°: applying pressure at an angle of 45° means that the direction of the pressure is partly vertical and partly horizontal. This way of applying pressure can promote the extension of bubbles in a specific direction to a certain extent, especially if the direction of the pressure is coordinated with the direction in which the bubbles need to extend. For example, if the bubbles need to extend in a plane of the mixture to form a long strip, the applied pressure should be inclined and partially directed in the normal direction of the plane, which can promote the extension of the bubbles in a plane parallel to the direction of the pressure.
[0223] To form a horizontally long elliptical bubble stack, theoretically, the direction of applied pressure should make the bubbles less affected by pressure in the horizontal direction and more affected by pressure in the vertical direction. Under such conditions, the bubbles tend to extend in the direction affected by relatively less pressure.
[0224] To achieve a specific elongated elliptical bubble, the angle at which pressure is applied may need to be adjusted based on the specific preparation conditions and material properties. Ideally, this angle may need to be optimized in the laboratory by adjusting the angle and observing changes in bubble morphology.
[0225] The best angle of inclination for applying pressure depends on many factors, including the viscosity of the raw materials, the rate of the foaming reaction, and the speed of rigid foam curing. In practical applications, applying pressure at a 45° angle can be used as a starting point, and experiments may involve gradual adjustments from this angle to find the best conditions to achieve the goal of forming long oval bubbles in the horizontal direction.
[0226] In short, by controlling the direction and magnitude of applied pressure, the bubble morphology of polyurethane rigid foam can be controlled to a certain extent, thereby affecting its thermal conductivity and other properties. Achieving this usually requires precise process control and condition optimization.
[0227] Furthermore, when the pressure chamber is pressurized, the mold in which the curing mold is located is vibrated;
[0228] Furthermore, the vibration frequency of the vibration treatment is between 20 Hz and 20,000 Hz. For example, it can be 20 Hz, 30 Hz, 40 Hz, 50 Hz, 80 Hz, 100 Hz, 200 Hz, 300 Hz, 500 Hz, 1000 Hz, 3000 Hz, 5000 Hz, 10000 Hz, 15000 Hz, 20000 Hz, etc.
[0229] In the above, the unit Hz is the number of vibrations per second, for example, 20 Hz means 20 vibrations per second.
[0230] In the present invention, it is known through experiments that a vibration frequency of 20 Hz-50 Hz, or reaching an ultrasonic level, that is, 20,000 Hz, can make the flat pressure bubbles in the material more evenly distributed.
[0231] It should be noted that in the preparation process of polyurethane rigid foam, applying pressure while vibrating the material at a certain frequency is an effective technical means to optimize the microstructure of the foam and improve its overall performance. This method is based on several key physical and chemical principles:
[0232] (1) Promote uniform distribution of bubbles
[0233] Vibration can help disperse bubbles formed in the polymer matrix and make them more evenly distributed. Introducing vibration into the polyurethane reaction mixture can break up large bubbles and promote the formation and uniform growth of bubble nuclei, thereby reducing the dispersion of bubble size and achieving a more consistent pore size distribution.
[0234] (2) Control bubble size and shape
[0235] By adjusting the frequency and intensity of the vibration, the size and shape of the bubbles can be controlled to a certain extent. The vibration causes the bubbles to be subjected to periodic pressure changes during their formation and growth, which helps to form smaller and more regular bubbles. Small, evenly distributed bubbles are particularly important for improving the thermal insulation properties and mechanical strength of the material.
[0236] (3) Improve mixing uniformity
[0237] Applying vibration helps improve the mixing uniformity of the raw material mixture. In the production process of polyurethane foam, uniformly mixed raw materials are the key to obtaining foam with consistent properties. Vibration can promote the uniform mixing of reactive components such as isocyanates and polyols, ensure the uniformity of chemical reactions, and thus improve the quality of the product.
[0238] (4) Accelerate chemical reactions
[0239] Vibration can speed up chemical reactions by providing mechanical energy. In some cases, vibration can help break the forces between molecules, making it easier for reactants to come into contact and react, thereby speeding up the rate of polymerization.
[0240] (5) Reduce defects and improve physical properties
[0241] By applying vibration, defects in polyurethane rigid foam, such as open cells, uneven bubble distribution and macropores, which may reduce the mechanical properties and thermal insulation properties of the material, can be effectively reduced. The uniform and stable bubble structure is conducive to improving the compressive strength and stiffness of the material while reducing the thermal conductivity.
[0242] In short, applying a certain frequency of vibration is an effective means to optimize the performance of polyurethane rigid foam. In the conventional technology of preparing polyurethane rigid foam, some materials are directly placed in a mold and pressed in contact by physical compression. Since the material itself is a mixture, there may be a certain degree of uneven mixing or fluidity, resulting in high concentration or more materials in some positions, and low concentration or less materials in some positions, resulting in uneven distribution of internal bubbles in the overall product during the pressing process. In the present invention, in view of this uneven distribution, a vibration technology that is more suitable for the overall process of the method of the present invention is adopted. By finely controlling the vibration parameters, the microstructure of the foam can be significantly improved, thereby improving its comprehensive performance, including thermal insulation, mechanical strength and processing performance. In the present invention, the vibration conditions are carefully optimized to ensure the best effect, so that under a specific air pressure method, a specific time condition, and a certain vibration frequency, the effect of ensuring the uniformity of bubbles in the material can be achieved, and the problem of uneven distribution of internal bubbles can be avoided.
[0243] In addition, the present invention also provides a polyurethane rigid foam material, which is prepared by the preparation method of the polyurethane rigid foam material as described above;
[0244] Furthermore, the bubbles in the polyurethane rigid foam material are flat pressure bubbles, which are in the shape of long ovals; the vertical height of the flat pressure bubbles is smaller than the horizontal length;
[0245] Furthermore, the diameter of the vertical cross section of the flat pressure bubble is not greater than 3000 nm;
[0246] Furthermore, the diameter d of the vertical cross section of the flat pressure bubble is 扁形压力泡 conform to:
[0247] 70nm<d 扁形压力泡 ≤3000nm.
[0248] The diameter d of the vertical cross section of the flat pressure bubble is 扁形压力泡Greater than 70nm and infinitely close to 70nm.
[0249] The narrowest diameter of the flat pressure bubble is greater than 70nm and infinitely close to 70 nanometers, which is achieved based on physical principles and experimental design. This value is mainly selected to utilize the Knudsen effect to reduce the gas thermal conductivity (λ g ).
[0250] The Knudsen effect occurs when the free path length of a gas is similar to the size of the container it is in. The free path of a gas is the average distance that gas molecules travel between adjacent collisions. Under normal conditions, this distance is very small, and the movement of gas molecules causes heat to be transferred through convection and conduction. However, when the gas is in a very small space, such as a micron or nanometer-scale bubble, the free path of the gas molecules can match or be larger than the size of the bubble, and then there are fewer collisions between gas molecules, and the thermal convection of the gas is reduced, resulting in a decrease in heat transfer efficiency.
[0251] The purpose of choosing 70 nanometers as the narrowest diameter of the flat pressure bubble is to ensure that the Knudsen effect is fully utilized in the foam material. This size is small enough that the heat convection of gas molecules through these flat spaces is significantly restricted, while not too small to be difficult to achieve using conventional material processing techniques. This size was chosen based on the understanding of gas molecular dynamics and considerations of material processing capabilities.
[0252] Achieving a flat pressure bubble with a minimum diameter of 70 nanometers usually requires sophisticated material handling and processing techniques, including: adjusting the type and amount of foaming agent to control the formation and growth of bubbles during the foaming process. Using external pressure or other physical means to change the shape of the bubble from a round shape to a flat ellipse. Precisely controlling processing environmental conditions (such as temperature and pressure) to optimize the use of the Knudsen effect.
[0253] In general, the selection and implementation of the value of 70 nanometers is based more on a deep understanding of the mechanisms that affect heat conduction and technical feasibility considerations. Through experiments and optimization of material processing, the design goals can be achieved, thereby achieving the effect of reducing the overall thermal conductivity and improving the insulation performance of the material.
[0254] In addition, reference Figure 4 The present invention also provides a system 100 for preparing a polyurethane rigid foam material, which is prepared based on the method for preparing a polyurethane rigid foam material as described above;
[0255] The preparation system 100 of the polyurethane rigid foam material comprises:
[0256] Pressure chamber 1, curing mold 2 and pressurizing equipment 3;
[0257] The curing mold 2 is provided with a mold cavity 21 for placing a liquid mixture 200 for preparing the polyurethane rigid foam material;
[0258] The curing mold 2 can be placed in the pressure chamber 1;
[0259] The pressurizing device 3 is connected to the pressure vessel 1 and can increase the pressure in the pressure vessel 1;
[0260] As mentioned above, one curing mold 2 or multiple curing molds 2 can be placed in the pressure chamber 1, and the pressure chamber 1 can be a complete chamber or an upper cover structure connected to the curing mold 2. By connecting with the curing mold 2, a accommodating space is formed, thereby pressurizing the curing mold 2 with gas.
[0261] Furthermore, the polyurethane rigid foam material preparation system 100 further includes a vibration device 4 connected to the curing mold 2;
[0262] As mentioned above, the vibration device 4 is used to provide vibration at a specific frequency to the connected curing mold 2 .
[0263] The vibration device 4 can be arranged at the lower end of the curing mold 2 and connected to the curing mold 2 through a snap, so that the curing mold 2 is fixed on the vibration platform of the vibration device 4. The vibration power is output through the motor inside, so that the liquid mixture 200 in the mold cavity 21 of the curing mold 2 can provide a certain frequency of vibration during the reaction process under pressurized conditions.
[0264] Furthermore, the polyurethane rigid foam material preparation system 100 further includes a pressurization angle adjustment device 5 disposed on the top of the pressure chamber 1;
[0265] The boost angle adjustment device 5 includes a fixed base 51 disposed on the top of the pressure chamber 1, an adjustment portion 52 connected to the fixed base 51 and disposed in the pressure chamber 1, and a pressure interface 53 disposed on the upper end of the fixed base 51;
[0266] The pressure interface 53 is connected to the boosting device 3 through a pipeline;
[0267] The adjusting portion 52 includes a horizontal rotation shaft 521 , an angle adjustment shaft 522 , and an output port 523 which are connected in sequence.
[0268] As mentioned above, the horizontal rotating shaft 521 can rotate in the horizontal direction, and the angle adjustment shaft 522 can adjust the output angle of the output port 523, so that pressurization can be achieved in the pressure chamber 1 by adjusting in various pressure directions.
[0269] It should be noted that the reference Figure 5, the preparation system 100 of the rigid polyurethane foam material may be provided with a central control device 6, which includes a bus 61, and a processor 62, a storage module 63 (such as a hard disk, a memory card, a data card, etc., for storing the operating system and the collected data, such as pressure, vibration frequency, angle, etc.), an input module 64 (such as a keyboard, a mouse, a console, a control button, a knob, a lever), an output module 65 (such as a display, a touch screen display), and a power supply module 66 (AC / DC power supply) connected through the bus 61.
[0270] A supercharging motor 31 is provided in the supercharging device 3; a vibration motor 41 is provided in the vibration device 4; in the supercharging angle adjusting device 5, a rotation motor 5211 connected to the horizontal rotation shaft 521 and an angle adjusting motor 5221 connected to the angle adjusting shaft 522 are provided. The supercharging motor 31, the vibration motor 41, the rotation motor 5211, and the angle adjusting motor 5221 are all connected to the processor 62 through the bus 61, so that under the control of the processor 62, the operation of the supercharging motor 31 can be started and / or adjusted, the vibration frequency can be adjusted, and the pressure application direction can be adjusted.
[0271] The present invention will be further described below through specific embodiments, but it should be understood that these embodiments are only used for more detailed description and should not be construed as limiting the present invention in any form.
[0272] Comparative experiment 1: Examine different polyurethane raw materials
[0273] In this embodiment, the raw material formula of the rigid polyurethane foam material is examined.
[0274] Table 1. Raw material formulas in the examples and comparative examples
[0275]
[0276]
[0277] Remarks: In the above table header, "Shi" is the abbreviation of "Example", and "Dui" is the abbreviation of "Comparative Example". For example, "Shi 1" is "Example 1", and "Dui 2" is "Comparative Example 2", and the same applies hereinafter.
[0278] Preparation method:
[0279] S1. According to the component parameters in Table 1, different liquid mixtures in the examples and comparative examples are prepared by using polyurethane raw materials;
[0280] S2. Pour the liquid mixture into the cavity of the curing mold for reaction;
[0281] S3, first detect and obtain the milky time and gel time corresponding to the liquid mixture; determine the time condition for pressurization in the pressure chamber according to the milky time and the gel time; based on the time condition, pressurize the pressure chamber so that the liquid mixture fills the mold cavity of the curing mold under absolute pressure, and the round bubbles in the liquid mixture form flat pressure bubbles, and the polyurethane rigid foam material is obtained after curing.
[0282] Table 2. Time parameters in the embodiments and comparative examples
[0283] time Real 1 Real 2 Reality 3 1 2 3 Milky Time T Milky 6 7 5 8 6 8 Gel time Tgel 58 60 65 59 59 60 The first calculation coefficient N 1.2 1.2 1.2 1.2 1.2 1.2 The second calculation coefficient M 1 1 1 1 1 1 Pressure value bar 1 1 1 1 1 1 Reaction standing time Treaction 7.2 8.4 6 9.6 7.2 9.6 Boost duration T ends 58 60 65 59 59 60
[0284] Horizontal test results:
[0285] The thermal conductivity of the materials prepared in the above Examples 1-3 and Comparative Examples 1-3 was tested, and the results are shown in the following table.
[0286] Table 3. Thermal conductivity results of the embodiments and comparative examples
[0287] Test items Real 1 Real 2 Reality 3 1 2 3 Material status qualified qualified qualified Failure Failure Failure Thermal conductivity w / m·k 0.0141 0.140 0.0139 0.0199 0.0189 0.0190
[0288] analyze:
[0289] (1) The thermal conductivity of the polyurethane rigid foam materials prepared in Examples 1-3 and Comparative Examples 1-3 was investigated. Examples 1-3 were prepared using the method and components of the present invention, and the overall formula of Comparative Examples 1-3 was basically the same as that of Example 2, except that no perfluoro-4-methyl-2-pentene and organic bismuth catalyst were added in Comparative Example 1; no perfluoro-4-methyl-2-pentene was added in Comparative Example 2; and no organic bismuth catalyst was added in Comparative Example 3.
[0290] (2) From the results in Table 3, it can be seen that the formulation, dosage and method provided by the present invention can form a polyurethane rigid foam material well under a certain reaction standing time and pressurization duration.
[0291] (3) In Comparative Examples 2 and 3, only one raw material, perfluoro-4-methyl-2-pentene or an organic bismuth catalyst, was added. In the test results, the thermal conductivity of Comparative Examples 2 and 3 was lower than that of Comparative Example 1. This indicates that whether perfluoro-4-methyl-2-pentene or an organic bismuth catalyst is used alone, the thermal conductivity of the material can be reduced to a certain extent, that is, the thermal insulation performance of the material can be slightly improved.
[0292] (4) However, the products prepared in Comparative Examples 2 and 3 are not able to prepare fully qualified rigid foam materials that meet the requirements of the present invention, and their thermal conductivity coefficients are increased to varying degrees.
[0293] (5) In Comparative Example 1, the two substances, perfluoro-4-methyl-2-pentene and the organic bismuth catalyst, were not added, and a qualified polyurethane rigid foam material could not be formed, and its thermal conductivity even reached 0.0199.
[0294] (6) The thermal conductivity of Examples 1 to 3 is significantly lower than that of Comparative Examples 2 and 3, indicating that when perfluoro-4-methyl-2-pentene and an organic bismuth catalyst are used together, the effect of reducing the thermal conductivity is better than the effect of using perfluoro-4-methyl-2-pentene or an organic bismuth catalyst alone. This effect is close to and exceeds the cumulative effect of using perfluoro-4-methyl-2-pentene or an organic bismuth catalyst alone, indicating that perfluoro-4-methyl-2-pentene and an organic bismuth catalyst do produce a synergistic effect when used together, which greatly reduces the thermal conductivity.
[0295] In the present invention, perfluoro-4-methyl-2-pentene (perfluoroolefin) and an organic bismuth catalyst are added to the raw materials used. It can be seen from experimental data that the perfluoroolefin and the organic bismuth catalyst have a certain synergistic effect.
[0296] It can be seen from the experimental data that the thermal conductivity of the materials prepared in Examples 1-3 (as a combined group) is significantly lower than that of each single-use group of Comparative Examples 2 and 3, and is significantly lower than that of Comparative Example 1 which does not use any of the raw materials of perfluoro-4-methyl-2-pentene and the organic bismuth catalyst. Moreover, the technical effects of the three combined groups, compared with the combination of the technical effects of the two single-use groups in the comparative example, all exceed the technical effects of the numerical combination of the two single-use groups, indicating that the addition of perfluoro-4-methyl-2-pentene (perfluoroolefin) and the organic bismuth catalyst in the present invention can produce a significant synergistic effect.
[0297] The synergistic effect between perfluoroolefins and organobismuth catalysts is mainly reflected in their joint promotion of the formation of polyurethane rigid foam and optimization of the foam's microstructure and macroscopic properties. This synergistic effect helps to achieve a more uniform and stable foam structure, improves the foam's mechanical properties, such as toughness and ductility, and also achieves energy conservation and consumption reduction in the preparation process.
[0298] Based on the above analysis, it can be considered that the combined use of perfluoro-4-methyl-2-pentene (perfluoroolefin) and organic bismuth catalyst has a significant synergistic effect in reducing the thermal conductivity of the material. Compared with the technical effects of using each separately, the combined use produces unexpectedly better thermal insulation performance. This shows that the invention has better performance and practical value in achieving improved thermal insulation performance of materials.
[0299] Comparative experiment 2: Investigating different time conditions and pressure values
[0300] In this embodiment, based on the formula in the above-mentioned embodiment 2, and after the milky time and gel time are detected, different time parameter conditions and pressure values are investigated in the embodiments and comparative examples.
[0301] The first group of experiments: First, different time conditions in the examples and comparative examples were investigated. On the premise that the formula and pressure values remained unchanged, examples 4-6 and comparative examples 4-9 were set, and the specific parameters were as follows:
[0302] Table 4, different time conditions in the examples and comparative examples
[0303]
[0304]
[0305] The second group of experiments: Then, the pressure values of different external boost pressures in the embodiments and comparative examples were investigated. Under the premise that the formulation and time conditions remained unchanged, the embodiments 7-9 and comparative examples 10-12 were set, and the specific parameters were as follows:
[0306] Table 5. Investigation of pressure values of different external boost pressures in the examples and comparative examples
[0307] Parameters Real 7 Actual 8 Actual 9 10 11 Milky time 6 6 6 6 6 Gel time 58 58 58 58 58 The first calculation coefficient 1.3 1.3 1.3 1.3 1.3 The second calculation coefficient 1.2 1.2 1.2 1.2 1.2 Reaction standing time 7.8 7.8 7.8 7.8 7.8 Boost duration 69.6 69.6 69.6 69.6 69.6 Pressure value bar 0.5 1 1.5 0 5
[0308] Experimental results:
[0309] For the materials prepared in the examples and comparative examples in the above two groups of experiments, the material state observation and thermal conductivity test were performed respectively, and the specific results are shown in the following table:
[0310] Table 6. Thermal conductivity results of the embodiments and comparative examples
[0311]
[0312] analyze:
[0313] In the first group of experiments, under the premise of fixing the formula, milky time, and gel time, the reaction standing time and pressurization duration were investigated. Among them, Examples 4-6 met the requirements of the correlation coefficient in the present invention. In Comparative Example 4, only the first calculated coefficient was lower than the lower limit; in Comparative Example 5, only the first calculated coefficient exceeded the upper limit, in Comparative Example 6, only the second calculated coefficient was lower than the lower limit, in Comparative Example 7, only the first calculated coefficient exceeded the upper limit, the two coefficients in Comparative Example 8 were both lower than the lower limit, and the two coefficients in Comparative Example 9 were both higher than the upper limit.
[0314] In the second set of experiments, the pressure values were investigated with all other parameters fixed. Examples 7-9 investigated different pressure values in accordance with the present invention, while the pressure value of Example 10 was lower than the lower limit, i.e., no pressurization was performed, while Example 11 used a pressure value exceeding the pressure value specified in the present invention for pressurization.
[0315] Comparative experiment 3: Investigating different pressure directions
[0316] refer to Figure 6 In this embodiment, the formula in the above-mentioned embodiment 2 is used, and after the milky time and gel time are detected and under fixed time conditions and pressure values, during the preparation process, different pressure directions are investigated through the embodiments and comparative examples.
[0317] Table 7. Different pressure directions and experimental results used in the examples and comparative examples
[0318] Parameters Actual 10 Real 11 Real 11 12 13 14 Pressure direction° 45 90 135 20 155 270 Material status qualified qualified qualified qualified Failure Failure Thermal conductivity w / m·k 0.0138 0.0134 0.139 0.0149 0.0151 0.0166
[0319] analyze:
[0320] In this embodiment, under the premise of fixing all other parameters, the pressure direction is investigated. Among them, Examples 10-12 are pressurized in the pressure directions defined in the present invention, which are 45°, 90° and 135° respectively, while the direction used in Comparative Example 12 is less than 45°, and the direction used in Comparative Example 13 is greater than 135°. In addition, a group of Comparative Example 14 is added, in which the pressure is applied in a closed pressure chamber in a direction opposite to the direction of the material therein, that is, the pressure is applied by exhausting gas upward, and the angle is 270°. The specific pressure direction during the test can be referred to Figure 6 shown.
[0321] From the results in the table, it can be seen that in the pressure chamber, the pressure direction is within the direction of 45°-135°, and a good state can be achieved. In addition, since the overall pressurization time is relatively short, it can be found that different pressurization directions have a more obvious effect on the bubble morphology of the material, and different bubble morphologies lead to different thermal conductivity coefficients. When the pressure direction is vertically downward at 90°, compared with other relatively inclined angles, the bubble shape is more likely to form a shuttle-shaped, flat oval-shaped long bubble, and its thermal conductivity coefficient is lower.
[0322] When the angle is more inclined, reaching 45°-135°, that is, Comparative Examples 12-14, the specific bubble shape in the material is not easy to present as a regular shuttle or flat oval long bubble, and its shape is not easy to form. In the specific pressurized environment, in Comparative Example 15, when the angle is increased by 270°, it can be seen from the thermal conductivity that the thermal conductivity is further increased. It can be inferred that (1) the pressure direction has a direct impact on the thermal conductivity of the material; (2) when the pressure direction is within the direction of 45°-135°, the material can achieve a better and lower thermal conductivity.
[0323] Comparative experiment 4: Investigating different vibration frequencies
[0324] In this embodiment, the formula in the above-mentioned embodiment 2 is used, and after the milky time and gel time are detected and under fixed time conditions and pressure values, during the preparation process, different vibration frequencies are investigated through the embodiments and comparative examples.
[0325] Table 8. Different vibration frequencies and experimental results used in the examples and comparative examples
[0326] Parameters Actual 10 Real 11 Real 12 15 16 Vibration frequency Hz 20 50 20000 0 50000 Thermal conductivity w / m·k 0.0130 0.0124 0.0148 0.0138 0.0198
[0327] analyze:
[0328] In comparative experiment 4, the vibration frequency was investigated under the premise of fixing all other parameters. Comparative Example 15 did not apply vibration, and Comparative Example 16 used vibration at a frequency of 50,000 Hz. Examples 10-12 used the vibration frequency range defined in the present invention, i.e., 20-20,000 Hz.
[0329] It can be seen from the data in the table that when a certain frequency of vibration is generated without vibration, the bubbles in the material are more evenly distributed, the chemical reaction is accelerated, and the bubbles are more likely to form spindle-shaped or flat long bubbles quickly and efficiently under a certain pressure, and the thermal conductivity will further decrease within the corresponding preparation time. However, when the vibration is too large, reaching 20,000 Hz or above, a large number of bubbles will be vibrated out of the material during material preparation, or the bubbles will be broken and not formed, resulting in the inability to retain regular long bubbles of a certain shape under a certain density in the material, which has a great impact on the thermal conductivity. For example, 20,000 Hz will increase the thermal conductivity to 0.0148 w / m·k, and when the vibration frequency reaches 50,000 Hz, the thermal conductivity of the material will be further increased to 0.270 w / m·k. It is expected that a large number of bubbles will be discharged through high-frequency vibration, and the remaining bubbles will also be broken and become round bubbles fixed in the material, thereby greatly increasing the thermal conductivity.
[0330] In summary, it can be seen from the experimental data that applying vibrations of a reasonable frequency within a certain range is an effective means to optimize the performance of polyurethane rigid foam. In the conventional technology for preparing polyurethane rigid foam, some materials are directly placed in a mold and pressed in contact by a physical compression method. Since the material itself is a mixture, there may be a certain degree of uneven mixing or fluidity, resulting in high concentration or more materials in some positions, and low concentration or less materials in some positions, resulting in uneven distribution of internal bubbles in the overall product during the pressing process. In the present invention, in view of this uneven distribution, a vibration technology that is more suitable for the overall process of the method of the present invention is adopted. By finely controlling the vibration parameters, the microstructure of the foam can be significantly improved, thereby improving its comprehensive performance, including thermal insulation, mechanical strength and processing performance. In the present invention, the vibration conditions are carefully optimized to ensure the best effect, so that the uniformity of bubbles in the material can be achieved under specific air pressure method, specific time conditions, and at a certain vibration frequency, avoiding the problem of uneven distribution of internal bubbles.
[0331] In summary, the preparation method of the polyurethane rigid foam material provided by the present invention combines physical methods with chemical technology. By non-contact pressurizing the prepared liquid mixture in a pressure chamber, the liquid mixture fills the curing mold under absolute pressure, and the round bubbles in the liquid mixture form flat pressure bubbles. After curing, the polyurethane rigid foam material is obtained, which can significantly reduce λg, λs, and λr, thereby obtaining a lower thermal conductivity. The preparation conditions and production environment are simple, the production consumables are small, the method steps are simple, and the production cost is greatly reduced. A more efficient, convenient, lower production cost, and higher efficiency production method and approach are provided for the preparation of polyurethane rigid foam materials.
[0332] The above are preferred implementation modes and corresponding embodiments of the present invention. It should be pointed out that, for those skilled in the art, without departing from the creative concept of the present invention, several modifications and improvements may be made, including but not limited to the adjustment of proportions, processes, dosages and reaction vessels, which all fall within the scope of protection of the present invention.
Claims
1. A method for preparing a polyurethane rigid foam material, characterized in that: include: A liquid mixture is obtained according to the polyurethane raw material; pouring the liquid mixture into a mold cavity of a curing mold for reaction; Placing the curing mold in a pressure chamber, detecting the milky time and gel time corresponding to the liquid mixture; determining the time condition for pressurization in the pressure chamber according to the milky time and gel time; Based on the time condition, the pressure chamber is pressurized so that the liquid mixture fills the mold cavity of the curing mold under absolute pressure, and the round bubbles in the liquid mixture are formed into flat pressure bubbles, and a polyurethane rigid foam material is obtained after curing; the time condition includes the reaction standing time and the pressurization duration; The reaction standing time is the time during which the liquid mixture is poured into the curing mold and allowed to stand for reaction; and when the reaction standing time ends, the standing is ended at the end time point and pressurization is started; The pressurization duration is the duration of starting pressurization and maintaining the pressurized state after the reaction standing time of pouring the liquid mixture into the curing mold for reaction ends; Wherein, the calculation method of the reaction standing time is: ; in, is the reaction standing time; is the milky time; is the first calculation coefficient, and its value range is 1.2-1.5; The calculation method of the boost duration is: ; in, is the boost duration; is the gel time; is the second calculation coefficient, and its value range is 0.8-1.6; When the pressure chamber is pressurized, the pressure direction of the external pressurization pressure applied by the pressurization device is at any angle within the range of 45°-135° relative to the upper surface of the liquid mixture in the curing mold; The bubble density of the round bubbles generated in the liquid mixture is 500 / cm 3 -1000pcs / cm 3 ; The diameter of the circular bubble is 10 μm-20 μm; the flat pressure bubble in the polyurethane rigid foam material is in the shape of an elongated ellipse; the height of the flat pressure bubble in the vertical direction is less than the length in the horizontal direction; the diameter of the vertical cross section of the flat pressure bubble is not greater than 3000 nm; the diameter d of the vertical cross section of the flat pressure bubble meets the following conditions: 70 nm < d ≤ 3000 nm; The polyurethane raw material comprises: a reaction composition, an isocyanate substance and a foaming agent; The reaction composition includes water, nanocellulose, ionic liquid, perfluoro-4-methyl-2-pentene, organic tin and organic bismuth catalysts; Wherein, the reaction composition includes the following components in parts by weight: Water 1-8; Nanocellulose 0.05-2.5; Ionic liquid 0.1-3.5; Perfluoro-4-methyl-2-pentene 0.5-2.5; Organic tin 0.1-0.6; Organic bismuth catalyst 0.1-0.5; Polyester polyol 10-30; Polyether polyol 45-89; The external boost pressure when pressurizing the pressure chamber is an absolute pressure; The pressure value of the external boost pressure is 0.5 bar-1.5 bar; When the pressure chamber is pressurized, the mold cavity of the curing mold is also subjected to vibration treatment; the vibration frequency of the vibration treatment is 20Hz-20000Hz.
2. The method for preparing a polyurethane rigid foam material according to claim 1, characterized in that: The reaction composition further includes the following components: Polyester polyols, polyether polyols, silicone oils and amine catalysts.
3. The method for preparing a polyurethane rigid foam material according to claim 2, characterized in that: The amine catalyst is selected from any one of cyclohexylamine, bis(2-dimethylaminoethyl) ether, triethylamine and N, N-dimethylbenzylamine.
4. The method for preparing a polyurethane rigid foam material according to claim 2, characterized in that: The reaction composition further includes the following components in parts by weight: Silicone oil 1-4; Amine catalysts 1-4.
5. The method for preparing a polyurethane rigid foam material according to claim 1, characterized in that: The blowing agent is selected from any one or more of pentane, neopentane, methyl formate, HFC-245fa, LBA, R600, R600a, R-152a, R-134a, R-1234yf, opteon 1100 / 1150, HCFO-1224yd, HCFO-1234ze, HCFO-1243zf, and HCFO-1233xf; The liquid mixture is prepared according to the polyurethane raw material, comprising: Taking each component in the reaction composition and mixing it to prepare the reaction composition; Dividing the foaming agent into two parts, namely a first foaming agent and a second foaming agent; Mixing the isocyanate substance and the first blowing agent to obtain a first mixed material; mixing the reaction composition with a second blowing agent to obtain a second mixed material; Among them, the ratio of the first mixture to the second mixture is: first mixture: second mixture = (1.0-1.8): (0.8-1.6); and, in the first mixture, based on the total amount being 100%, the isocyanate substance accounts for 70%-100%; the first foaming agent is the balance; in the second mixture, based on the total amount being 100%, the reaction composition accounts for 70%-100%; the second foaming agent is the balance; the first mixture and the second mixture are mixed to obtain the liquid mixture.
6. A polyurethane rigid foam material, characterized in that: Prepared by the preparation method of the polyurethane rigid foam material according to any one of claims 1 to 5; The bubbles in the polyurethane rigid foam material are flat pressure bubbles, which are in the shape of long ovals; the vertical height of the flat pressure bubbles is smaller than the horizontal length; The diameter of the vertical cross section of the flat pressure bubble is not greater than 3000nm; The diameter d of the vertical cross section of the flat pressure bubble meets the following requirements: 70nm<d≤3000nm.
7. A system for preparing a polyurethane rigid foam material, characterized in that: Prepared based on the preparation method of the polyurethane rigid foam material according to any one of claims 1 to 5; The preparation system of the polyurethane rigid foam material comprises: Pressure chambers, curing moulds and pressurising equipment; The curing mold is provided with a mold cavity for placing the liquid mixture for preparing the polyurethane rigid foam material; The curing mold can be placed in the pressure chamber; The pressurizing device is connected to the pressure chamber and can increase the pressure in the pressure chamber.
8. The system for preparing polyurethane rigid foam material according to claim 7, characterized in that: The preparation system of the polyurethane rigid foam material also includes a vibration device connected to the curing mold.
9. The system for preparing polyurethane rigid foam material according to claim 7, characterized in that: The polyurethane rigid foam material preparation system further includes a pressurization angle adjustment device disposed on the top of the pressure chamber; The boost angle adjustment device comprises a fixed base arranged on the top of the pressure chamber, an adjustment part connected to the fixed base and placed in the pressure chamber, and a pressure interface arranged on the upper end of the fixed base; The pressure interface is connected to the boosting device via a pipeline; The adjustment part includes a horizontal rotation axis, an angle adjustment axis and an output port which are connected in sequence.
Citation Information
Patent Citations
Molded polyurethane bodies with excellent flexibility at low temperatures
CN107428908A
Reactive composition, polyurethane foam prepared from reactive composition and preparation method
CN117659490A