Carbon-coated non-graphitizable carbon, negative electrode for lithium-ion secondary battery, and lithium-ion secondary battery

By optimizing the thickness and orientation of the carbon coating layer in the negative electrode material of the lithium ion secondary battery, and combining the parameter optimization of the electron diffraction method and the electron energy loss spectroscopy method, the problem of low charging and discharging efficiency of carbon materials in the existing technology is solved. Achieving both high discharge capacity and initial efficiency.

CN118139814BActive Publication Date: 2024-10-29JFE CHEMICAL CORP +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380013947.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2024-10-29
Estimated Expiration
2043-06-26

AI Technical Summary

Technical Problem

In the existing technology, the orientation degree of the carbon material and the thickness distribution of the coating layer are not fully considered, resulting in the negative electrode material of the lithium ion secondary battery being unable to obtain sufficient discharge capacity and initial efficiency under charge and discharge conditions.

Method used

By setting the average thickness of the carbon coating layer in the carbon-coated non-graphitizable carbon to be 4 nm or more and 30 nm or less, and ensuring that the minimum value of the thickness is more than 70% of the maximum value, combined with the selected area electron diffraction method and the electron energy loss spectroscopy method The parameters are optimized to ensure that the diffraction intensity and layer spacing of the carbon coating meet specific conditions to take into account high discharge capacity and initial efficiency.

Benefits of technology

It achieves both high discharge capacity and initial efficiency in the negative electrode material of lithium ion secondary battery, and improves the charge and discharge efficiency and life characteristics of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118139814B_ABST
    Figure CN118139814B_ABST
Patent Text Reader

Abstract

The subject of the present invention is to provide a carbon-coated non-graphitizable carbon that can achieve both high discharge capacity and initial efficiency when used for a negative electrode for a lithium ion secondary battery, a negative electrode for a lithium ion secondary battery using the carbon-coated non-graphitizable carbon, and a lithium ion secondary battery having the negative electrode for a lithium ion secondary battery. The carbon-coated non-graphitizable carbon of the present invention comprises non-graphitizable carbon and a carbon coating layer coated on its surface, the average thickness of the carbon coating layer is greater than 4 nm and less than 30 nm, and the minimum value of the thickness of the carbon coating layer is greater than 70% of the maximum value of the carbon coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to carbon-coated non-graphitizable carbon, a negative electrode for a lithium ion secondary battery, and a lithium ion secondary battery. Background Art

[0002] In recent years, due to the improvement of global awareness of the protection of the earth's environment, in order to reduce the use of fossil fuels and reduce CO2 emissions, power generation using renewable energy has gradually become popular. Renewable energy generated by solar power generation, wind power generation, etc. is easily affected by time period, season, climate, etc. Therefore, by making full use of the energy storage system (Energy Storage System, hereinafter also referred to as "ESS") for suppressing output fluctuations, the stabilization of power supply can be achieved. Large-scale batteries are required for power storage systems. Therefore, lithium-ion secondary batteries (LIBs) with high energy density per unit volume and mass and capable of being miniaturized have attracted much attention. At present, carbon materials are generally used as negative electrode materials for lithium-ion secondary batteries. In addition to carbon, lithium salts of metals or metal oxides such as Si, Sn, Ti, V, etc., and mixed materials of carbon and metals with high energy density are in the research stage.

[0003] Among carbon materials, graphite materials generally have high capacity and have been widely used in portable electronic devices, etc., but for ESS applications, non-graphitizable carbon materials with high charge and discharge capacity and cycle characteristics are suitable. In particular, unlike batteries for hybrid vehicles, ESS applications strongly require a charge capacity that can be charged to a large capacity at a low charge rate and a lifespan that can be repeatedly charged and discharged for a long time.

[0004] Regarding the difficult graphitization carbon material as the negative electrode material of the lithium ion secondary battery, it is characterized in that it is formed by non-oriented graphene layer units, has a crystallite diameter smaller than that of the graphite material, and has pores between the graphene layer units. Due to these structural features, Li can be absorbed and released not only between the layers but also in the pores, so it can be known that compared with the theoretical capacity of graphite 372mAh / g, the difficult graphitization carbon material has a higher discharge capacity. In addition, since the crystallite diameter of the graphene layer unit is small and non-oriented, the volume change accompanying the insertion / extraction of Li is also small compared with the graphite material, and the life characteristics are also excellent. However, since the crystallite is small, the graphene edge with a large amount of reaction activity reacts with the electrolyte to form a SEI (Solid Electrolyte Interphase, solid electrolyte interface) film, so the initial efficiency expressed as the percentage of the initial discharge capacity relative to the charge capacity is low and becomes a problem.

[0005] As a method for improving initial efficiency, a method of coating the surface of a carbon material is known. Patent Document 1 discloses a non-aqueous electrolyte secondary battery, which uses a carbon material having a structure in which the surface of a substrate carbon material is coated with a coating carbon material in the negative electrode, characterized in that the (002) plane of the coating carbon material based on the X-ray wide-angle diffraction method is oriented parallel to the surface of the substrate carbon material, and the orientation degree is 70% or more. In addition, it is disclosed that the thickness of the surface carbon layer is preferably (angstrom).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 10-233206 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, the orientation degree of the carbon material of patent document 1 is obtained by image analysis from a range of 20nm from the surface, and the distribution of the orientation in the thickness direction is not considered. In addition, the distribution of the thickness of the coated carbon material is not considered. Moreover, when the inventors of the present invention used the carbon material of patent document 1 for the negative electrode of a lithium ion secondary battery, it was clear that sufficient discharge capacity and initial efficiency could not be obtained according to the charge and discharge conditions.

[0011] The present invention is completed in view of the above situation, and its purpose is to provide a carbon-coated non-graphitizable carbon that can achieve both high discharge capacity and initial efficiency when used for a negative electrode for a lithium ion secondary battery, a negative electrode for a lithium ion secondary battery using the above-mentioned carbon-coated non-graphitizable carbon, and a lithium ion secondary battery having the above-mentioned negative electrode for a lithium ion secondary battery.

[0012] Solution to the problem

[0013] The present inventors have studied a structure that can achieve both discharge capacity and initial efficiency, and the results show that in carbon-coated non-graphitizable carbon, when the carbon coating layer has a given average thickness and a uniform thickness, both high discharge capacity and initial efficiency can be achieved.

[0014] That is, the present inventors have found that the above-mentioned problems can be solved by the following configuration.

[0015] (1) A carbon-coated non-graphitizable carbon, comprising non-graphitizable carbon and a carbon coating layer coated on the surface of the non-graphitizable carbon,

[0016] The average thickness of the carbon coating layer is greater than or equal to 4 nm and less than or equal to 30 nm.

[0017] The minimum thickness of the carbon coating layer is greater than 70% of the maximum thickness of the carbon coating layer.

[0018] (2) The carbon-coated non-graphitizable carbon according to (1) above, wherein

[0019] In the diffraction intensity of the carbon coating layer obtained by selected area electron diffraction,

[0020] The peak intensity Ix corresponding to the 002 plane of graphite in the tangential direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula (1).

[0021] Ix / Iy<1.00 (1)

[0022] (3) The carbon-coated non-graphitizable carbon according to (1) or (2) above, wherein:

[0023] In the diffraction pattern of the carbon coating layer measured by selected area electron diffraction,

[0024] The interlayer spacing d002 of the 002 plane obtained from the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is 0.38 nm or more.

[0025] (4) The carbon-coated non-graphitizable carbon according to any one of (1) to (3) above, wherein

[0026] The Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy is greater than 0.090, where Isp2 is the intensity of the peak derived from sp2, and Isp3 is the intensity of the peak derived from sp3.

[0027] (5) A carbon-coated non-graphitizable carbon, comprising non-graphitizable carbon and a carbon coating layer coated on the surface of the non-graphitizable carbon,

[0028] The average thickness of the carbon coating layer is greater than or equal to 4 nm and less than or equal to 30 nm.

[0029] The minimum thickness of the carbon coating layer is more than 70% of the maximum thickness of the carbon coating layer.

[0030] In the diffraction intensity of the carbon coating layer obtained by the selected area electron diffraction method, the peak intensity Ix corresponding to the 002 plane of graphite in the tangential direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula (1):

[0031] In the diffraction pattern of the carbon coating layer measured by selected area electron diffraction, the interlayer spacing d002 of the 002 plane obtained from the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is 0.38 nm or more,

[0032] The Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy is greater than 0.090, where Isp2 is the intensity of the peak derived from sp2, and Isp3 is the intensity of the peak derived from sp3.

[0033] Ix / Iy<1.00 (1)

[0034] (6) The carbon-coated non-graphitizable carbon according to any one of (1) to (5) above, wherein

[0035] The diffraction pattern of the non-graphitizable carbon measured by selected area electron diffraction does not have a peak corresponding to the 002 plane of the graphite structure.

[0036] (7) A carbon-coated non-graphitizable carbon, comprising non-graphitizable carbon and a carbon coating layer coated on the surface of the non-graphitizable carbon,

[0037] The average thickness of the carbon coating layer is greater than or equal to 4 nm and less than or equal to 30 nm.

[0038] The minimum thickness of the carbon coating layer is more than 70% of the maximum thickness of the carbon coating layer.

[0039] In the diffraction intensity of the carbon coating layer obtained by the selected area electron diffraction method, the peak intensity Ix corresponding to the 002 plane of graphite in the tangential direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula (1):

[0040] In the diffraction pattern of the carbon coating layer measured by selected area electron diffraction, the interlayer spacing d002 of the 002 plane obtained from the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is 0.38 nm or more,

[0041] The Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy is greater than 0.090,

[0042] In the diffraction pattern of the non-graphitizable carbon measured by selected area electron diffraction, no peak corresponding to the 002 plane of the graphite structure was observed.

[0043] Here, Isp2 is the intensity of the peak derived from sp2, and Isp3 is the intensity of the peak derived from sp3.

[0044] Ix / Iy<1.00 (1)

[0045] (8) A negative electrode for a lithium ion secondary battery, comprising the carbon-coated non-graphitizable carbon according to any one of (1) to (7).

[0046] (9) A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to (8) above.

[0047] Effects of the Invention

[0048] As shown below, according to the present invention, there can be provided a carbon-coated non-graphitizable carbon that can achieve both high discharge capacity and initial efficiency when used for a negative electrode for a lithium ion secondary battery, a negative electrode for a lithium ion secondary battery using the above-mentioned carbon-coated non-graphitizable carbon, and a lithium ion secondary battery having the above-mentioned negative electrode for a lithium ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 This is a diagram showing an example of a peak corresponding to the 002 plane.

[0050] Figure 2 It is a cross-sectional view showing a coin-type secondary battery for evaluation.

[0051] Explanation of symbols

[0052] 1. External cup

[0053] 2 Working electrode

[0054] 3 Outer cans

[0055] 4 pairs of electrodes

[0056] 5. Partition

[0057] 6 Insulation pad

[0058] 7a Current Collector

[0059] 7b Current Collector DETAILED DESCRIPTION

[0060] Hereinafter, the carbon-coated non-graphitizable carbon, the negative electrode for a lithium ion secondary battery, and the lithium ion secondary battery of the present invention will be described.

[0061] In addition, the numerical range expressed using "to" in this specification means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0062] In addition, each component may be used alone or in combination of two or more. Here, when two or more components are used in combination, the content of the components refers to the total content unless otherwise specified.

[0063] Furthermore, when used for a negative electrode for a lithium ion secondary battery, the fact that a high discharge capacity and a high initial efficiency are exhibited is also simply referred to as “excellent effects of the present invention”.

[0064] [1] Carbon-coated non-graphitizable carbon

[0065] The carbon-coated non-graphitizable carbon of the present invention is a carbon-coated non-graphitizable carbon (carbon material) comprising non-graphitizable carbon and a carbon coating layer coated on the surface thereof (hereinafter, also referred to as “the carbon material of the present invention”).

[0066] The average thickness of the carbon coating layer is 4 nm or more and 30 nm or less.

[0067] The minimum value of the thickness of the carbon coating layer is not less than 70% of the maximum value of the carbon coating layer.

[0068] When the surface of the non-graphitizable carbon is active and used as the negative electrode of a Li-ion battery, it reacts with the electrolyte and Li during charging to form a reaction layer, which reduces efficiency. The carbon-coated non-graphitizable carbon of the present invention has a carbon coating layer, which reduces surface reactivity, inhibits solvent decomposition, and improves efficiency and storage durability. By uniformly coating, efficiency can be improved without hindering the absorption and release of Li.

[0069] In addition, during repeated charge and discharge, conductivity cannot be ensured between particles of the non-graphitizable carbon, and particles that do not function as active materials increase, thereby reducing efficiency. The carbon-coated non-graphitizable carbon of the present invention improves surface conductivity through the carbon coating layer, prevents the conductive path from being cut off, and improves efficiency.

[0070] [Difficult to graphitize carbon]

[0071] The hardly graphitizable carbon of the carbon material of the present invention is a type of amorphous carbon, which is carbon that is hardly graphitized even by heat treatment, and conventionally known hardly graphitizable carbon can be appropriately used.

[0072] [Carbon coating]

[0073] The carbon coating layer of the carbon material of the present invention is a layer covering the surface of the non-graphitizable carbon and is mainly composed of carbon atoms. The carbon is amorphous carbon (hard carbon, soft carbon), graphite, or a mixture of amorphous carbon and graphite.

[0074] [thickness]

[0075] <Average Thickness>

[0076] The carbon coating layer has an average thickness of 4 nm to 30 nm.

[0077] When the above-mentioned average thickness is less than 4nm, there is a non-coated portion locally and the effect of efficiency improvement cannot be obtained. Therefore, the average thickness is set to more than 4nm, and from the reason that the effect of the present invention is more excellent, it is preferably more than 7nm. When the above-mentioned average thickness exceeds 30nm, when used as the negative electrode of a Li ion secondary battery, the occlusion and release of Li will be hindered and the effect of efficiency improvement cannot be obtained. Therefore, the average thickness is set to less than 30nm, and from the reason that the effect of the present invention is more excellent, it is preferably less than 20nm, and more preferably less than 15nm.

[0078] The average thickness of the carbon coating layer can be obtained by STEM (Scanning Transmission Electron Microscope) observation of a particle cross section.

[0079] Select particles of average particle size of carbon-coated difficult-graphitizing carbon, perform carbon vapor deposition or gold vapor deposition on the flat part of the particle, and process it into a thin sheet of less than 140nm at room temperature by focused ion beam (FIB) in a way that the vertical cross section of the carbon coating layer can be observed. Observe the vertical cross section of the carbon coating layer by STEM, and measure the thickness of the carbon coating layer in the bright field (Bright field; BF) image of any field of view. Measure the thickness of 5 places separated by more than 50nm, and find the average thickness. Since the crystal orientation of the carbon coating layer is different from that of the difficult-graphitizing carbon, the carbon coating layer can be distinguished by the lattice stripes of the BF image, and the thickness can be measured. When distinguishing the carbon coating layer from the difficult-graphitizing carbon, the contrast difference of the annular dark field (Annular Dark Field; ADF) image and the crystal orientation difference of the FFT (Fast Fourier Transform) can also be used as an auxiliary combination to make a judgment.

[0080] <Minimum / Maximum>

[0081] The minimum value of the thickness of the above-mentioned carbon coating layer is more than 70% of the maximum value of the above-mentioned carbon coating layer. Hereinafter, the ratio of the minimum value of the carbon coating layer to the maximum value of the carbon coating layer is also referred to as "minimum value / maximum value". The larger the minimum value / maximum value, the higher the uniformity of the thickness of the carbon coating layer. That is, in the carbon material of the present invention, the uniformity of the thickness of the carbon coating layer is high.

[0082] In the carbon material of the present invention, by uniformly coating the carbon coating layer, the occlusion and release of Li will not be hindered, and the efficiency can be improved. When the minimum value / maximum value is less than 70%, the occlusion and release of Li become uneven, and the efficiency decreases. The upper limit is not particularly limited, but it is difficult to control to more than 98%.

[0083] From the perspective of achieving more excellent effects of the present invention, the minimum value / maximum value ratio is preferably 75% or more, more preferably 80% or more, further preferably 85% or more, and particularly preferably 90% or more.

[0084] The minimum / maximum value can be obtained by observing a vertical cross section of the carbon coating layer produced by the above method using STEM and measuring the maximum and minimum values ​​of the carbon coating layer in an arbitrarily selected 200 nm square range in a BF image of an arbitrary field of view.

[0085] [Appropriate method]

[0086] [Ix / Iy]

[0087] For the carbon material of the present invention, because the effect of the present invention is more excellent, among the diffraction intensity of the carbon coating layer obtained by the selected area electron diffraction method, it is preferred that the peak intensity Ix corresponding to the 002 plane of graphite in the tangent direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula.

[0088] Ix / Iy<1.00 (1)

[0089] When Ix / Iy is less than 1.00, the c-axis of the carbon is oriented along the normal direction of the carbon coating. When used as a battery, the reactive graphene edge is not easily in contact with the electrolyte, which can inhibit the decomposition of the electrolyte and further improve the initial efficiency.

[0090] When Ix / Iy is 1.00 or more, the c-axis orientation is insufficient and the effect of improving efficiency is small. The lower limit of Ix / Iy is not particularly limited, but it is difficult to set it to 0.10 or less.

[0091] Ix and Iy can be obtained by the selected area electron diffraction method of the carbon coating. The vertical section of the carbon coating made by the above method is observed by TEM, and the selected area electron diffraction pattern of the carbon coating is obtained in the range of 100nm of diameter centered on the carbon coating. According to the line profile of the tangent direction of the carbon coating of the obtained Debye ring and the normal direction of the carbon coating, the peak intensity of the peak corresponding to the 002 surface is set to Ix and Iy respectively. It should be noted that, since the crystal orientation of the carbon coating is different from that of the difficult graphitized carbon, the carbon coating can be distinguished according to the difference in contrast of the TEM image.

[0092] Figure 1 An example of a peak corresponding to the 0002 plane is shown. The horizontal axis is the position from the center of the Debye ring in the reciprocal lattice space, and the vertical axis is the brightness (intensity) of the Debye ring. The inverse of the peak position of the peak corresponding to the 002 plane is the interlayer spacing d002.

[0093] [Layer interval d002]

[0094] Because the effect of the present invention is more excellent, in the diffraction pattern of the carbon coating layer of the carbon material of the present invention measured by selected area electron diffraction, the layer spacing d002 of the 002 plane obtained based on the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is preferably greater than 0.38 nm.

[0095] By setting d002 to 0.38 nm or more, the increase or decrease of the interlayer spacing of the 002 surface accompanying the occlusion and release of Li is mitigated, and the initial efficiency is further improved. When d002 is less than 0.38 nm, the interlayer spacing of the 002 surface accompanying the occlusion and release of Li changes, and the effect of improving efficiency is small. There is no upper limit for d002, but it is difficult to set it to 0.45 nm or more.

[0096] d002 can be obtained by selected area electron diffraction, and can be obtained based on the position of the peak corresponding to the 002 plane.

[0097] [Isp2 / (Isp2+Isp3)]

[0098] From the reason that the effect of the present invention is more excellent, the carbon material of the present invention preferably has an Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy of 0.090 or more. The carbon c-axis with high Isp2 / (Isp2+Isp3) is oriented along the normal direction of the carbon coating layer. When used as a battery, the reactive graphene edge is not easy to contact the electrolyte, the decomposition of the electrolyte is suppressed, and the initial efficiency can be further improved. When Isp2 / (Isp2+Isp3) is less than 0.090, the orientation is insufficient and the effect of improving the efficiency is small. The upper limit of Isp2 / (Isp2+Isp3) is not particularly limited, but it is difficult to control it above 0.130.

[0099] Isp2 / (Isp2+Isp3) can be obtained by electron energy loss spectroscopy. The vertical cross section of the carbon coating layer is subjected to linear analysis based on electron energy loss spectroscopy at a spacing of 0.5 nm in the normal direction of the carbon coating layer, and the intensity Isp2 of the peak from sp2 near the loss energy 286eV and the intensity Isp3 of the peak from sp3 near the loss energy 397eV are obtained. The highest Isp2 / (Isp2+Isp3) in the normal direction of the carbon coating is taken as the Isp2 / (Isp2+Isp3) of the carbon coating layer.

[0100] [Peak of the 002 plane of the graphite structure of the non-graphitizable carbon]

[0101] From the reason that the effect of the present invention is more excellent, the carbon material of the present invention preferably does not have a peak corresponding to the 002 surface of the graphite structure in the diffraction pattern of the substrate (difficult to graphitize carbon) measured by the selected area electron diffraction method. In the case where the graphite structure is not developed, the peak equivalent to the 002 surface becomes a broad peak and cannot be judged as a peak. In the case where the graphite structure is not developed, the sites of Li occlusion and release from the pores increase, and a higher discharge capacity can be obtained.

[0102] The presence or absence of the peak corresponding to the 002 plane of the graphite structure is confirmed by the selected area electron diffraction method in the STEM observation of the particle cross section. Specifically, the presence or absence of the peak corresponding to the 002 plane of the graphite structure is confirmed by the selected area electron diffraction method inside the particle 50nm or more from the interface between the non-graphitizable carbon and the carbon coating layer.

[0103] The method of controlling the peak corresponding to the 002 plane of the graphite structure is not particularly limited. For example, by setting the calcination temperature of the non-graphitizable carbon to 650° C. or higher and 850° C. or lower, non-graphitizable carbon having no peak corresponding to the 002 plane of the graphite structure can be obtained.

[0104] [Impurities in the carbon coating]

[0105] The carbon coating layer preferably does not contain impurity elements. When the carbon coating layer contains elements such as H, N, O, P, S, and metal elements such as Si, Fe, Zn, Al, and Mg, it will react with Li to form a compound when used as a battery, and the initial efficiency will decrease. The content of impurities can be confirmed by TEM-EDX (energy dispersive X-ray spectroscopy), and preferably the elements other than C are below the detection limit.

[0106] [Average particle size]

[0107] From the viewpoint of obtaining a thick-film electrode coating with a large capacity, the average particle size of the carbon material of the present invention is preferably 15 to 40 μm or less, and more preferably 20 to 35 μm.

[0108] It should be noted that the average particle size of the carbon material of the present invention is the particle size (D 50 ).

[0109] [Specific surface area]

[0110] In the carbon material of the present invention, the specific surface area (BET) obtained by the BET method based on nitrogen adsorption varies depending on the particle size and cannot be generalized, but from the reason of suppressing the reactivity with the electrolyte, it is preferably 10 m 2 / g or less, more preferably 0.10 to 6.0 m 2 / g.

[0111] [2] Method for producing carbon-coated non-graphitizable carbon

[0112] The carbon-coated non-graphitizable carbon of the present invention (the carbon material of the present invention) can be obtained, for example, by the following production method. It should be noted that the production method for obtaining the carbon material of the present invention is not limited to the following method.

[0113] [Manufacturing of non-graphitizable carbon]

[0114] [Cross-linking treatment]

[0115] First, a raw material of non-graphitizable carbon (hereinafter, also simply referred to as "raw material") is subjected to a cross-linking treatment to obtain a cross-linked product.

[0116] Here, as raw materials, there is no particular limitation, and existing known raw materials can be used, for example, asphalts such as coal-based asphalt and petroleum-based asphalt; resins such as phenolic resins and furan resins; mixtures of asphalt and resins, etc. Among them, from the viewpoint of economy, asphalts such as coal-based asphalt and petroleum-based asphalt are preferred. In particular, by using coal-based asphalt, the 002 plane spacing (layer spacing d002) of difficult graphitizable carbon is easily within the above range, so it is preferred.

[0117] Examples of methods for crosslinking the raw materials include: methods based on air blowing reaction; dry methods based on oxidizing gas (air, oxygen, ozone); wet methods using aqueous solutions of nitric acid, sulfuric acid, hypochlorous acid, mixed acid, etc. Among them, methods based on air blowing reaction are preferred.

[0118] The air blowing reaction is a reaction in which the softening point is raised by heating the above raw materials and blowing an oxidizing gas (e.g., air, oxygen, ozone, or a mixture thereof). According to the air blowing reaction, a cross-linked product (e.g., air-blown asphalt) having a high softening point of, for example, 200° C. or higher can be obtained.

[0119] It should be noted that it is known that the air blowing reaction is a reaction in a liquid phase state, and compared with the cross-linking treatment in a solid phase state, oxygen atoms are basically not incorporated into the carbon material.

[0120] In the blowing reaction, an oxidative dehydration reaction is carried out as the main reaction, and polymerization is carried out through biphenyl-type cross-linking bonds. Then, through subsequent infusibility and sintering (described later), the cross-linked portion has a three-dimensional structure with no dominant orientation, and a large amount of pores for absorbing and releasing lithium can be obtained.

[0121] The conditions of the air blowing reaction are not particularly limited. Since an intermediate phase is generated when the temperature is too high and the reaction rate is slow when the temperature is low, the reaction temperature is preferably 280 to 420°C, and more preferably 320 to 380°C. In addition, the blowing amount of the oxidizing gas is preferably 0.5 to 15 L (liters) / minute per 1000 g of asphalt in terms of compressed air, and more preferably 1.0 to 10 L / minute. The reaction pressure may be any of normal pressure, reduced pressure, and pressurized pressure, and is not particularly limited.

[0122] The softening point of the cross-linked product such as air-blown pitch obtained by such a cross-linking treatment is preferably 200 to 400°C, more preferably 250 to 350°C, from the perspective of ease of infusibility treatment.

[0123] The obtained cross-linked product may be coarsely pulverized using an atomizer or the like before being subjected to the infusibility treatment.

[0124] [Infusible treatment]

[0125] Next, the cross-linked product such as the air-blown asphalt is subjected to an infusible treatment to obtain an infusible product (e.g., infusible asphalt). The infusible treatment is a cross-linking treatment (oxidation treatment) performed in a solid phase, whereby oxygen is incorporated into the structure of the cross-linked product, and further cross-linking is performed to make it difficult to melt at high temperatures.

[0126] There are no particular limitations on the method of infusibility treatment, and examples thereof include a dry method using an oxidizing gas (air, oxygen); a wet method using an aqueous solution of nitric acid, sulfuric acid, hypochlorous acid, a mixed acid, etc. Among these, a dry method using an oxidizing gas is preferred.

[0127] The treatment temperature for the infusibility treatment should be selected to be below the softening point of the cross-linked product. In order to further prevent fusion, the heating rate during batch treatment is preferably 5 to 100°C / hour, more preferably 10 to 50°C / hour.

[0128] The other treatment conditions in the infusibility treatment are not particularly limited. For example, the blowing amount of the oxidizing gas is preferably 1.0 to 20 L / min, more preferably 2.0 to 10 L / min per 1000 g of compressed air. The reaction pressure may be any of normal pressure, reduced pressure, and pressurized pressure, and is not particularly limited.

[0129] The oxygen content of the infusible product obtained by the infusible treatment is preferably 3 to 20% by mass, more preferably 5 to 15% by mass, from the viewpoint of preventing fusion during firing.

[0130] [Crushing treatment]

[0131] Next, the infusible product such as infusible asphalt is pulverized to adjust the particle size.

[0132] At this time, the average particle size of the infusible product after the pulverization treatment is preferably 15 to 40 μm, and more preferably 20 to 35 μm. It should be noted that the average particle size here refers to the particle size (D 50 ).

[0133] The pulverizer used for the pulverization treatment is not particularly limited, and a conventionally known pulverizer can be used. Examples thereof include a jet mill, a pin mill, a ball mill, a hammer mill, a roll mill, and a vibration mill.

[0134] When using these pulverizers, the pulverization conditions are set so that the average particle size of the infusible product after the pulverization process falls within the above-mentioned range.

[0135] [Firing]

[0136] Next, the infusible treated product such as the infusible pitch after the pulverization treatment is fired in a reduced pressure or inert gas atmosphere such as nitrogen to obtain non-graphitizable carbon. The firing temperature (firing temperature) is 600 to 1200° C., preferably 650 to 850° C. At this time, the heating rate is preferably 50 to 150° C. / hour, more preferably 80 to 120° C. / hour.

[0137] [Formation of Carbon Coating Layer]

[0138] The method for forming the carbon coating layer is not particularly limited, and a method based on chemical vapor deposition (CVD: Chemical Vapor Deposition) can be cited. In order to form a carbon coating layer with uniform thickness, high sp2 orientation, and specific 002 plane spacing (layer spacing d002), it is very important to form the carbon coating layer by thermal decomposition after the raw material molecules evenly reach the substrate, which can be achieved by a method corresponding to the diffusibility and thermal decomposition characteristics of the raw material molecules.

[0139] Low molecular weight methane and acetylene with high diffusivity can form a uniform carbon coating layer in an appropriate temperature range and an appropriate concentration range by a thermal CVD method of a flow system. Depending on the type of gas used, the suitable temperature is different. In the case of methane, the temperature range of the carbon substrate is preferably 800-1000°C. When it is lower than 800°C, the thermal decomposition is insufficient and it is difficult to form a carbon coating layer. When it exceeds 1000°C, the thermal decomposition in the gas phase is promoted to generate coal, which will become an uneven carbon coating layer. The concentration range is preferably 10-80% by volume. When it is less than 10% by volume, the supply of raw materials is insufficient, and the formation of the carbon coating layer will take time. When it exceeds 80% by volume, the thermal decomposition in the gas phase is sometimes promoted to generate coal, which will become an uneven carbon coating layer. In the case of acetylene, the temperature range of the carbon substrate is preferably 600-800°C. When it is lower than 600°C, the thermal decomposition is insufficient and it is difficult to form a carbon coating layer. When it exceeds 800°C, the thermal decomposition in the gas phase is promoted to generate coal, which will become an uneven carbon coating layer. The concentration range is preferably 10 to 80% by volume. When it is less than 10% by volume, the supply of raw materials is insufficient and the formation of the carbon coating layer takes time. When it exceeds 80% by volume, thermal decomposition in the gas phase is sometimes promoted to generate coal, thereby forming an uneven carbon coating layer. The temperature of the introduced methane and acetylene and the temperature of the inert gas diluting these gases are preferably room temperature.

[0140] On the other hand, raw materials with large molecular weight and low diffusivity can form a uniform carbon coating layer by CVI (Chemical Vapor Infiltration), which is a type of CVD (Chemical Vapor Deposition). That is, the sintered difficult-to-graphitize carbon is heated to 700-1100°C in a vacuum gas atmosphere, the carbon source is introduced into the furnace in the form of gas and maintained at a pressure of 1-30 kPa for 1 second to 30 seconds, and the carbon source is removed by exhausting. Then, the carbon source is introduced again, and by repeating it many times, a carbon-coated difficult-to-graphitize carbon material coated with pyrolytic carbon can be obtained. The carbon source is any carbon source that produces carbon by pyrolysis. When the carbon source is liquid at room temperature, it is introduced by gasifying it at a temperature above the boiling point. For example, benzene, hexane, toluene, cyclohexane, etc. can be used. Depending on the raw material, the appropriate temperature is different, especially from the viewpoint of being easy to decompose at low temperatures and easily forming pyrolytic carbon, and obtaining a uniform and highly oriented carbon coating layer, cyclohexane is preferably used as the carbon source. A carbon source that is liquid at room temperature is preheated in a gas atmosphere of 100 to 200°C and introduced into the furnace in the form of a gas. Since it is not instantly vaporized at temperatures below 100°C, the gas distribution in the furnace becomes uneven and the carbon coating becomes uneven. When heated to more than 200°C, depending on the type of liquid carbon source, decomposition sometimes occurs before coating, making the carbon coating uneven. At 100 to 200°C, thermally decomposable carbon that can stably coat non-graphitizable carbon can be introduced into the furnace. When a carbon source that is liquid at room temperature is used, it is easier to control the supply to the furnace and can be introduced in large quantities compared to a carbon source that is gaseous at room temperature, so it is preferred.

[0141] For raw materials with large molecular weight and low diffusivity, especially carbon sources that are liquid at room temperature, when using a thermal CVD method of a circulation system without using CVI, inert gases such as N2, Ar, and He that have been cooled to below 10°C are bubbled at a certain flow rate in a carbon source liquid that has been cooled to below 10°C and introduced into the furnace. In the thermal CVD method of the circulation system, when the concentration of the carbon source contained in the introduced gas increases, the carbon source is carbonized before coating and partially attached to the difficult-to-graphitize carbon, or the growth rate of the coating is too fast and the film thickness is locally thickened, so it is easy to form a film with uneven film thickness. By cooling the carbon source that is bubbled, the carbon concentration in the gas becomes thin, and a stable and uniform film thickness can be formed. As a carbon source, for example, benzene, hexane, toluene, cyclohexane, etc. can be used. Depending on the raw material, the appropriate temperature is different, especially from the perspective of being easy to decompose at low temperatures and easily forming thermally decomposable carbon, and obtaining a uniform and highly oriented carbon coating layer, cyclohexane is preferably used as the carbon source.

[0142] Although the heat treatment temperature (coating treatment temperature) is limited by the thermal decomposition temperature of the carbon source, it is preferably above 600°C and below 1100°C. When the heat treatment temperature is lower than 600°C, the introduced carbon source does not undergo thermal decomposition, and a thermally decomposable carbon coating cannot be obtained, and the initial efficiency is sometimes reduced. When the heat treatment temperature exceeds 1100°C, the structure of the difficult graphitizable carbon is changed by calcining during the heat treatment, and sometimes the desired initial capacity cannot be obtained. The heat treatment temperature is preferably below the calcination temperature of the difficult graphitizable carbon so that the difficult graphitizable carbon does not undergo structural changes.

[0143] [3] Lithium-ion secondary battery

[0144] Next, a lithium ion secondary battery (hereinafter also referred to as “lithium ion secondary battery of the present invention”) using the carbon-coated non-graphitizable carbon of the present invention (carbon material of the present invention) as a negative electrode material will be described.

[0145] Lithium-ion secondary batteries usually have negative electrodes, positive electrodes, and non-aqueous electrolytes as their main battery components. The positive and negative electrodes are respectively formed of substances (as layered compounds) or compounds or clusters that can absorb and release lithium ions, and the entry and exit of lithium ions during the charge and discharge process occurs between the layers. It is a battery mechanism in which lithium ions are doped into the negative electrode during charging and dedoped from the negative electrode during discharge.

[0146] The lithium ion secondary battery of the present invention is not particularly limited except that the carbon-coated non-graphitizable carbon of the present invention is used as a negative electrode material, and other battery components are based on the components of a general lithium ion secondary battery.

[0147] [negative electrode]

[0148] The method for manufacturing a negative electrode from the carbon-coated non-graphitizable carbon of the present invention is not particularly limited and can be carried out according to a conventional manufacturing method. When manufacturing a negative electrode, a negative electrode mixture formed by adding a binder to the carbon-coated non-graphitizable carbon of the present invention can be used. As a binder, it is preferred to use a binder that has chemical stability and electrochemical stability relative to the electrolyte, and it is usually preferably used in an amount of about 1 to 20% by mass in the total amount of the negative electrode mixture. As a binder, polyvinylidene fluoride, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), etc. can be used. In addition, as an active material, carbon materials and graphite materials other than the carbon-coated non-graphitizable carbon of the present invention can be added. As a conductive agent, for example, carbon black, carbon fiber, etc. can be added.

[0149] The carbon-coated non-graphitizable carbon of the present invention is mixed with a binder to prepare a paste-like negative electrode mixture coating, which is usually applied to one or both sides of the collector to form a negative electrode mixture layer. At this time, a common solvent can be used in the preparation of the coating. The shape of the collector used for the negative electrode is not particularly limited, and examples thereof include: foil; mesh, porous metal and other meshes. Examples of the collector include copper, stainless steel, nickel and the like.

[0150] [positive electrode]

[0151] As the positive electrode material (positive electrode active material), it is preferred to select a material that can be doped / dedoped with a sufficient amount of lithium ions. Examples of such positive electrode active materials include transition metal oxides, transition metal chalcogenides, vanadium oxides, and lithium-containing compounds thereof, and compounds of the general formula M X 6S 8-Y (wherein, X is a value in the range of 0≤X≤4, Y is a value in the range of 0≤Y≤1, and M represents a metal such as a transition metal) represented by a Chevreul phase compound, lithium iron phosphate, activated carbon, activated carbon fiber, etc. They can be used alone or in combination of two or more. For example, carbonates such as lithium carbonate can also be added to the positive electrode.

[0152] The lithium-containing transition metal oxide is a composite oxide of lithium and a transition metal, or may be an oxide formed by solid solution of lithium and two or more transition metals. Specifically, the lithium-containing transition metal oxide is LiM(1) 1-P M(2) P O2 (wherein P is a value in the range of 0≤P≤1, and M(1) and M(2) are composed of at least one transition metal element), or LiM(1) 2-Q M(2) Q O4 (wherein Q is a numerical value in the range of 0≤Q≤1, and M(1) and M(2) are composed of at least one transition metal element). Here, as the transition metal element represented by M, Co, Ni, Mn, Cr, Ti, V, Fe, Zn, Al, In, Sn, etc. can be cited, preferably Co, Fe, Mn, Ti, Cr, V, Al. Such lithium-containing transition metal oxides can be obtained by using, for example, Li, oxides or salts of transition metals as starting materials, mixing these starting materials according to the composition, and calcining them in an oxygen atmosphere at a temperature range of 600 to 1000°C. It should be noted that the starting materials are not limited to oxides or salts, and can also be synthesized from hydroxides, etc.

[0153] As a method for forming a positive electrode using such a positive electrode material, for example, a positive electrode mixture layer is formed by applying a paste-like positive electrode mixture coating formed by a positive electrode material, a binder and a conductive agent to one or both sides of a collector. As a binder, the binders exemplified in the negative electrode can be used. As a conductive agent, for example, particulate carbon materials, fibrous carbon materials, graphite, carbon black, VGCF (vapor grown carbon fiber) can be used. The shape of the collector is not particularly limited, and the same shape as the negative electrode can be used. As the material of the collector, aluminum, nickel, stainless steel foil, etc. can usually be used.

[0154] When forming the above-mentioned negative electrode and positive electrode, various additives such as conventionally known conductive agents and binders may be appropriately used.

[0155] [Electrolytes]

[0156] As the electrolyte, a common non-aqueous electrolyte containing a lithium salt such as LiPF6, LiBF4, etc. as an electrolyte salt can be used.

[0157] The non-aqueous electrolyte may be a liquid non-aqueous electrolyte solution, or may be a polymer electrolyte such as a solid electrolyte or a gel electrolyte.

[0158] In the case of a liquid nonaqueous electrolyte solution, an aprotic organic solvent such as ethylene carbonate, propylene carbonate, or dimethyl carbonate can be used as the nonaqueous solvent.

[0159] In the case of a polymer electrolyte, a matrix polymer after gelation with a plasticizer (non-aqueous electrolyte) is included. As the matrix polymer, ether polymers such as polyethylene oxide and its crosslinked products, polymethacrylates, polyacrylates, polyvinylidene fluoride, fluorine-based polymers such as vinylidene fluoride-hexafluoropropylene copolymers, etc. can be used alone or in combination, wherein, from the viewpoint of redox stability, etc., fluorine-based polymers are preferably used.

[0160] As the electrolyte salt and the non-aqueous solvent constituting the plasticizer (non-aqueous electrolyte solution) contained in the polymer electrolyte, those that can be used for liquid electrolyte solutions can be used.

[0161] In the lithium ion secondary battery of the present invention, microporous bodies of polypropylene and polyethylene or materials made of them into layer structures are generally used; separators such as non-woven fabrics. Gel electrolytes can also be used. In this case, for example, a negative electrode (negative electrode for lithium ion secondary battery of the present invention) using carbon-coated non-graphitizable carbon of the present invention, a gel electrolyte, and a positive electrode are stacked in sequence and contained in a battery outer packaging material.

[0162] The structure of the lithium ion secondary battery of the present invention is arbitrary, and its shape and form are not particularly limited, and it can be arbitrarily selected from, for example, a cylindrical shape, a square shape, and a coin shape.

[0163] Example

[0164] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto.

[0165] [Example 1]

[0166] [Manufacturing of non-graphitizable carbon]

[0167] <Cross-linking treatment>

[0168] 1000 g of coal-based QI-free (quinoline insoluble component) pitch (QI: 0.1-0.5 mass %, softening point: 82.5° C.) was placed in an autoclave equipped with an anchor-type stirring device and heated to 320° C. under a nitrogen stream. Then, compressed air was blown into the pitch while flowing at 2 L / min and heated at 320° C. for 2 hours to perform a crosslinking treatment based on an air blowing reaction. Then, the mixture was cooled to room temperature and the contents (air-blown pitch) were taken out.

[0169] <Infusible treatment>

[0170] Next, the air-blown asphalt was roughly crushed with an atomizer, put into a rotary furnace, and heated at 20°C / hour while circulating compressed air at 2 L / min, and maintained at 250°C for 3 hours to perform an infusible treatment, thereby obtaining infusible asphalt.

[0171] <Crushing>

[0172] The obtained infusible pitch was pulverized using a jet mill (FS-4, manufactured by Seishin Enterprise Co., Ltd.) under conditions such that the average particle size of the pulverized product became 29 μm.

[0173] <Firing>

[0174] 100 g of the pulverized infusible pitch was placed in a graphite covered container, heated to a calcination temperature of 750° C. at a heating rate of 100° C. / hour under a nitrogen flow, and calcined at 750° C. for 2 hours to obtain carbon powder. The obtained carbon powder was a powder of non-graphitizable carbon.

[0175] [Formation of Carbon Coating Layer]

[0176] Next, the obtained carbon powder was placed in a tubular furnace and heated to 750°C at a temperature rise rate of 5°C / min at a pressure of 1kPa. Then, while maintaining the temperature at 750°C (coating treatment temperature), toluene was preheated in a gas atmosphere of 200°C and introduced into the tubular furnace. Then, after maintaining the pressure at 10kPa for 15 seconds, the gas was exhausted until the pressure was 1kPa. By repeating the above operation 30 times, a carbon coating layer was formed on the surface of the difficult graphitizable carbon. Thus, carbon-coated difficult graphitizable carbon was obtained.

[0177] [Example 2]

[0178] Carbon-coated non-graphitizable carbon was obtained by the same procedure as in Example 1 except that the pulverization conditions were changed and the calcination temperature and coating temperature were changed to 850°C.

[0179] [Example 3]

[0180] Carbon-coated non-graphitizable carbon was obtained by the same procedure as in Example 1 except that the pulverization conditions were changed, the calcination temperature and the coating treatment temperature were changed to 700° C., and cyclohexane was used instead of toluene.

[0181] [Example 4]

[0182] A non-graphitizable carbon powder was obtained by following the same procedure as in the production of non-graphitizable carbon in Example 1 except that the calcination temperature was changed to 700°C.

[0183] Next, the obtained carbon powder was placed in a tubular furnace, heated to 700°C at a heating rate of 5°C / min under N2 gas flow, and maintained at 700°C. Then, N2 gas at 5°C was bubbled in cyclohexane maintained at 5°C, and N2 gas containing cyclohexane was introduced into the furnace and maintained for 60 minutes. Then, it was cooled. Thus, a carbon coating layer was formed on the surface of the difficult graphitizable carbon, and a carbon-coated difficult graphitizable carbon was obtained.

[0184] [Comparative Example 1]

[0185] Carbon powder was obtained by the same procedure as that for producing non-graphitizable carbon in Example 1 except that the pulverization conditions were changed and the calcination temperature was changed to 1100° C. In Comparative Example 1, no carbon coating layer was formed.

[0186] [Comparative Example 2]

[0187] Carbon powder was obtained by the same procedure as in Example 1 for producing non-graphitizable carbon, except that the pulverization conditions were changed and the calcination temperature was changed to 850° C. In Comparative Example 2, no carbon coating layer was formed.

[0188] [Comparative Example 3]

[0189] Carbon-coated non-graphitizable carbon was obtained by following the same procedure as in Example 1 except that the pulverization conditions were changed and the calcination temperature and coating temperature were changed to 700°C.

[0190] [Comparative Example 4]

[0191] First, the pulverization conditions were changed and the calcination temperature was changed to 850°C. In addition, carbon powder was obtained by following the same steps as those for the manufacture of the difficult-graphitizing carbon in Example 1. The obtained carbon powder is a powder of difficult-graphitizing carbon. Next, the obtained carbon powder was placed in a tubular furnace, heated to 850°C at a heating rate of 5°C / min under a flow of N2 gas, and maintained at 850°C. Then, N2 gas at 50°C was bubbled in toluene maintained at 50°C, and the N2 gas containing toluene was introduced into the furnace and maintained for 60 minutes. Then, it was cooled. Thus, a carbon coating layer was formed on the surface of the difficult-graphitizing carbon, and carbon-coated difficult-graphitizing carbon was obtained.

[0192] [Comparative Example 5]

[0193] A non-graphitizable carbon powder was obtained by following the same procedure as in the production of non-graphitizable carbon in Example 1 except that the calcination temperature was changed to 700°C.

[0194] Next, benzene was used instead of toluene as a carbon precursor (carbon source), the bubbling temperature was set to 15°C (the temperatures of benzene and N2 gas were both set to 15°C), and the holding temperature was set to 800°C. In addition, a carbon coating layer was formed on the surface of the non-graphitizable carbon according to the same steps as in Comparative Example 4 to obtain carbon-coated non-graphitizable carbon.

[0195] [Comparative Example 6]

[0196] A non-graphitizable carbon powder was obtained by following the same procedure as in the production of non-graphitizable carbon in Example 1 except that the calcination temperature was changed to 700°C.

[0197] Next, benzene was used instead of toluene as a carbon precursor (carbon source), the bubbling temperature was set to 15°C (the temperatures of benzene and N2 gas were both set to 15°C), and the holding temperature was set to 1000°C. In addition, a carbon coating layer was formed on the surface of the non-graphitizable carbon according to the same steps as in Comparative Example 4 to obtain carbon-coated non-graphitizable carbon.

[0198] [evaluate]

[0199] [Evaluation of Carbon Powder]

[0200] First, the carbon powder obtained in Examples 1 to 4 and Comparative Examples 1 to 6 was subjected to STEM and TEM observation of the powder cross section. The average thickness of the carbon coating layer, the maximum and minimum values ​​of the thickness of the carbon coating layer, Ix / Iy of the carbon coating layer, the interlayer spacing d002 of the carbon coating layer, Isp2 / (Isp2+Isp3) of the carbon coating layer, and the presence or absence of a peak corresponding to the 002 surface of the substrate (difficult to graphitize carbon) were determined by the above method. The results are shown in Tables 1 to 2 below. It should be noted that STEM and TEM observations were performed using JEM-ARM200F manufactured by JEOL Ltd. and observed at an accelerating voltage of 200 kV.

[0201] The average particle size is the particle size when the cumulative frequency of the laser diffraction particle size distribution analyzer is 50% in terms of volume percentage (D 50 ). The specific surface area was obtained by the BET method based on nitrogen adsorption.

[0202] [Battery evaluation]

[0203] Next, using the carbon powders obtained in Examples 1 to 4 and Comparative Examples 1 to 6 as negative electrode materials, coin-type secondary batteries for evaluation were prepared (refer to Figure 2 ), and various evaluations were conducted.

[0204] <Preparation of Negative Electrode Mixture Paste>

[0205] First, the obtained carbon powder was used as the negative electrode material to prepare a negative electrode mixture paste. Specifically, carbon powder (95 parts by mass) and a 12% N-methylpyrrolidone solution of polyvinylidene fluoride (5 parts by mass in terms of solid content) were placed in a planetary mixer, stirred at 100 rpm (round per minute) for 15 minutes, and N-methylpyrrolidone was further added to adjust the solid content ratio to 60%, and stirring was continued for 15 minutes to prepare a negative electrode mixture paste.

[0206] <Preparation of working electrode (negative electrode)>

[0207] The prepared negative electrode mixture paste was applied to the copper foil in a uniform thickness, and then placed in a blower dryer to volatilize the solvent at 100°C to form a negative electrode mixture layer. Next, the negative electrode mixture layer was pressurized using a roller press and further punched into a circle with a diameter of 15.5 mm, thereby producing a working electrode (negative electrode) having a negative electrode mixture layer that was closely attached to the collector formed by the copper foil. It should be noted that before evaluation, drying was performed at 100°C in a vacuum for more than 8 hours.

[0208] <Preparation of Electrolyte>

[0209] In a mixed solvent of ethylene carbonate (33 vol%) and ethyl methyl carbonate (67 vol%), LiPF6 was added at a concentration of 1 mol / dm 3 The concentration of was dissolved to prepare a non-aqueous electrolyte.

[0210] <Production of Evaluation Battery>

[0211] Next, using the prepared working electrode (negative electrode), Figure 2 The coin-type secondary battery for evaluation (also simply referred to as "evaluation battery") is shown. Figure 2 is a cross-sectional view showing a coin-type secondary battery for evaluation.

[0212] First, a lithium metal foil was pressed against a nickel mesh and punched out into a circle with a diameter of 15.5 mm, thereby producing a disk-shaped counter electrode 4 made of lithium foil in close contact with a current collector 7 a made of the nickel mesh.

[0213] Next, the separator 5 impregnated with the electrolyte solution was sandwiched between the working electrode (negative electrode) 2 in close contact with the current collector 7b and the counter electrode 4 in close contact with the current collector 7a, and the working electrode 2 was then contained in the outer cup 1, the counter electrode 4 was contained in the outer can 3, the outer cup 1 and the outer can 3 were joined, and the edges of the outer cup 1 and the outer can 3 were riveted and sealed with an insulating gasket 6 interposed therebetween, thereby manufacturing an evaluation cell.

[0214] In the manufactured evaluation battery, the edges of the outer cup 1 and the outer can 3 are riveted with an insulating pad 6 sandwiched therebetween to form a sealed structure. Figure 2 As shown, the current collector 7a, the counter electrode 4, the separator 5, the working electrode (negative electrode) 2 and the current collector 7b are stacked in this order from the inner surface of the outer can 3 toward the inner surface of the outer cup 1.

[0215] <Charge and discharge test>

[0216] The produced evaluation battery was subjected to the following charge and discharge test at 25° C. In this test, the process of doping lithium ions into carbon powder is referred to as “charge”, and the process of dedoping lithium ions from carbon powder is referred to as “discharge”.

[0217] First, a constant current charge is performed at a current value of 0.39mA until the circuit voltage reaches 0mV, and a constant voltage charge is switched to the moment when the circuit voltage reaches 0mV, and further, the charge is continued until the current value reaches 20μA. The first charge capacity (unit: mAh / g) is obtained based on the amount of power supplied during this period. Then, stop for 120 minutes. Next, a constant current discharge is performed at a current value of 0.39mA until the circuit voltage reaches 1.5V, and a constant voltage discharge is switched to the moment when the circuit voltage reaches 1.5V, and further, the discharge is continued until the current value reaches 20μA. The first discharge capacity (unit: mAh / g) is obtained based on the amount of power supplied during this period. The results are shown in Tables 1 to 2. In practice, the discharge capacity is preferably 540mAh / g or more.

[0218] From the results of the above charge and discharge test, the initial efficiency (unit: %) was calculated based on the following formula. The results are shown in Tables 1 and 2. In practical terms, the initial efficiency is preferably 78% or more.

[0219] Initial efficiency = (first discharge capacity / first charge capacity) × 100

[0220] For Example 4 and Comparative Example 2, the absolute value of the voltage change before and after the discharge was completed without current flowing for 10 minutes was evaluated as the IR drop (unit: V). Example 4 was 0.14 V, and Comparative Example 2 was 0.18 V. The smaller the IR drop, the smaller the internal resistance of the battery, and the higher average voltage as a battery can be obtained, and a stable conductive path can be obtained, so the cycle characteristics are excellent.

[0221]

[0222]

[0223] As shown in Tables 1 and 2, Examples 1 to 4 in which the average thickness of the carbon coating layer was 4 nm to 30 nm and the minimum / maximum value of the thickness of the carbon coating layer was 70% or more all showed high discharge capacity and high initial efficiency.

[0224] On the other hand, in Comparison Examples 1 to 2 without a carbon coating, Comparison Examples 3 to 6 with a carbon coating but a minimum / maximum value of the thickness of the carbon coating less than 70%, an average thickness of the carbon coating exceeding 30 nm or an average thickness less than 4 nm, at least one of the discharge capacity or the initial efficiency is insufficient.

Claims

1. A carbon-coated non-graphitizable carbon, comprising non-graphitizable carbon and a carbon coating layer coated on the surface thereof, The average thickness of the carbon coating layer is greater than or equal to 4 nm and less than or equal to 30 nm. The minimum thickness of the carbon coating layer is greater than 70% of the maximum thickness of the carbon coating layer.

2. The carbon-coated non-graphitizable carbon according to claim 1, wherein: In the diffraction intensity of the carbon coating layer obtained by selected area electron diffraction, The peak intensity Ix corresponding to the 002 plane of graphite in the tangential direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula (1): Ix / Iy<1.00 (1).

3. The carbon-coated non-graphitizable carbon according to claim 1, wherein: In the diffraction pattern of the carbon coating layer measured by selected area electron diffraction, The interlayer spacing d002 of the 002 plane obtained from the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is 0.38 nm or more.

4. The carbon-coated non-graphitizable carbon according to claim 1, wherein: The Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy is greater than 0.090, wherein Isp2 is the intensity of the peak from sp2, and Isp3 is the intensity of the peak from sp3.

5. A carbon-coated non-graphitizable carbon, comprising non-graphitizable carbon and a carbon coating layer coated on the surface thereof, The average thickness of the carbon coating layer is greater than or equal to 4 nm and less than or equal to 30 nm. The minimum thickness of the carbon coating layer is more than 70% of the maximum thickness of the carbon coating layer. In the diffraction intensity of the carbon coating layer obtained by the selected area electron diffraction method, the peak intensity Ix corresponding to the 002 plane of graphite in the tangential direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula (1): Ix / Iy<1.00 (1) In the diffraction pattern of the carbon coating layer measured by selected area electron diffraction, the interlayer spacing d002 of the 002 plane obtained from the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is 0.38 nm or more, The Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy is greater than 0.090, wherein Isp2 is the intensity of the peak from sp2, and Isp3 is the intensity of the peak from sp3.

6. The carbon-coated non-graphitizable carbon according to claim 1, wherein: The diffraction pattern of the non-graphitizable carbon measured by selected area electron diffraction does not have a peak corresponding to the 002 plane of the graphite structure.

7. A carbon-coated non-graphitizable carbon, comprising non-graphitizable carbon and a carbon coating layer coated on the surface thereof, The average thickness of the carbon coating layer is greater than or equal to 4 nm and less than or equal to 30 nm. The minimum thickness of the carbon coating layer is more than 70% of the maximum thickness of the carbon coating layer. In the diffraction intensity of the carbon coating layer obtained by the selected area electron diffraction method, the peak intensity Ix corresponding to the 002 plane of graphite in the tangential direction of the carbon coating layer and the peak intensity Iy corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer satisfy the following formula (1): Ix / Iy<1.00 (1) In the diffraction pattern of the carbon coating layer measured by selected area electron diffraction, the interlayer spacing d002 of the 002 plane obtained from the peak corresponding to the 002 plane of graphite in the normal direction of the carbon coating layer is 0.38 nm or more, The Isp2 / (Isp2+Isp3) of the carbon coating layer measured by electron energy loss spectroscopy is greater than 0.090, wherein Isp2 is the intensity of the peak from sp2, and Isp3 is the intensity of the peak from sp3. In the diffraction pattern of the non-graphitizable carbon measured by selected area electron diffraction, no peak corresponding to the 002 plane of the graphite structure was observed. 8 . A negative electrode for a lithium ion secondary battery, comprising the carbon-coated non-graphitizable carbon according to claim 1 . 9 . A lithium ion secondary battery comprising the negative electrode for a lithium ion secondary battery according to claim 8 .

Citation Information

Patent Citations

  • Negative pole material for lithium ion secondary battery, negative pole for lithium ion secondary battery, and lithium ion secondary battery

    CN103098274A

  • High-capacity ratio rate carbon-based composite material, preparation method thereof and application thereof in lithium ion battery

    CN107768626A

  • Hardly graphitizable carbonaceous material for nonaqueous electrolyte secondary batteries used in fully charged state, method for producing same, negative electrode material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery in fully charged state

    CN107925082A

  • Lithium ion secondary battery negative electrode material and lithium ion secondary battery

    CN110998927A

  • Hard carbon negative electrode composite material and preparation method and application thereof

    CN113184827A