Tantalum coating and preparation method thereof
The tantalum and copper element are synchronously deposited by chemical vapor deposition method to form a composite copper element coating with tantalum element as the matrix, which solves the problem of clinical surgical infection and improves the bone tissue repair effect, and achieves the synergistic efficiency of tantalum and copper metal. Ensures the biocompatibility and mechanical properties of the material.
Patent Information
- Application Number
- CN202410152212.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-03
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-03
AI Technical Summary
Existing medical bone implant materials have problems intraoperative infection and postoperative infection in clinical surgery, and the composite deposition method of tantalum metal coating causes copper element to cover tantalum element, which cannot exert the synergistic effect of the two metals, affecting the Bone tissue repair.
The chemical vapor deposition method is used to synchronize the deposition of tantalum and copper elements, and a composite copper element coating with tantalum elements as the matrix is formed on the surface of the matrix material. The argon and nitrogen atmosphere control ensure that both metals can come into contact with human tissues and regulate them. Cells behave and have antibacterial properties.
It improves the biocompatibility and antibacterial properties of bone implant materials, enhances the bone tissue repair effect, avoids the problem of uneven deposition, and ensures the adaptability and mechanical properties of the coating to human tissue.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of medical bone implant materials, and more specifically, to a tantalum coating and a preparation method thereof. Background Art
[0002] In recent years, the number of patients with bone defects caused by trauma, congenital diseases and other reasons has increased. When the bone defect is large, it cannot rely on the regeneration of human bone tissue for self-repair, and needs to be repaired with the help of medical bone implant materials. Therefore, people have an increasing demand for medical bone implant materials. Medical bone implant materials are mainly used to repair and fill bone defects or fix and support fracture ends, including autologous bone, allogeneic bone, metal materials, polymer materials, inorganic non-metallic materials, etc. As human implants, medical bone implant materials should have good biocompatibility, bioaffinity and human safety; they should have a certain strength in mechanics, and their mechanical properties should be compatible with human bone tissue, with an elastic modulus close to that of human bones, and they should also be wear-resistant and aging-resistant; chemically, they should have stable performance, corrosion resistance and be easy to disinfect and sterilize.
[0003] Preparing a coating with excellent performance on the surface of bone implant materials is an effective way to improve the performance of bone tissue materials. Chemical vapor deposition, magnetron sputtering, plasma spraying, etc. are currently commonly used coating preparation methods. Among the current methods for preparing bone implant materials, chemical vapor deposition technology is the implant material preparation technology with the highest feasibility for industrial production because of its low process difficulty, simple operation, high yield rate, and chemical vapor deposition technology is the most stable and most suitable for industrial production.
[0004] Tantalum, as an emerging bio-implantable metal, has strong corrosion resistance and excellent osteogenic activity. It can effectively combine with human bone tissue and has better tissue repair performance than titanium. However, problems such as intraoperative infection and postoperative infection in clinical surgery are still very serious, affecting the quality and effect of clinical surgery. The method of preparing medical metal tantalum coating with chemical vapor deposition technology has the advantages of simple preparation, low energy consumption, and large-scale production. The development of antibacterial functional bone implant material tantalum coating can effectively improve the applicability of bone tissue and improve the effect of clinical surgery.
[0005] A Chinese patent with publication number CN116837343A discloses a method for preparing copper-plated medical tantalum metal materials by chemical vapor deposition. Tantalum pentachloride is generated by reacting pure tantalum with chlorine, and the tantalum pentachloride is replaced with hydrogen to obtain a tantalum element deposited on the surface of a substrate; pure tantalum is replaced with pure copper to react with chlorine, and then replaced with hydrogen to obtain a copper element deposited on the surface of the tantalum element. This technical solution retains the advantages of tantalum metal and has a simple preparation method. However, the tantalum element is replaced first, and then copper element is deposited on the surface of the tantalum element. This multi-layer deposition method allows the copper element to cover the first layer of tantalum element, and human tissues and cells can only contact the outermost layer of copper element metal, and the synergistic effect of tantalum and copper cannot be exerted. Summary of the invention
[0006] In order to solve the above technical problems, the present application provides a preparation method for depositing a tantalum coating on the surface of a base material by chemical vapor deposition and a tantalum coating obtained by the preparation method. Through the preparation method, tantalum and copper are deposited simultaneously to form a tantalum coating with a tantalum base and a composite copper base on the surface of the base material with a synergistic effect, thereby solving the problem of easy infection in clinical surgery and improving the bone defect treatment effect of medical bone implant materials.
[0007] The technical solution adopted in this application is as follows: a method for preparing a tantalum coating is provided, comprising the following steps:
[0008] (1) reacting solid pure tantalum metal with chlorine to obtain tantalum pentachloride gas, and then conveying the tantalum pentachloride gas into a reaction chamber of a CVD device containing a substrate material through argon gas, wherein the reaction chamber of the CVD device is filled with a high-purity argon gas atmosphere;
[0009] (2) Add cupric chloride powder into a quartz boat and place it in a quartz tube of a tube furnace. After evacuating the quartz tube, introduce nitrogen gas and heat it to obtain cupric chloride gas. The cupric chloride gas is introduced into the reaction chamber of the CVD equipment.
[0010] (3) Hydrogen is introduced into the reaction chamber of the CVD equipment to simultaneously displace tantalum and copper, and tantalum and copper are simultaneously deposited on the surface of the substrate material;
[0011] (4) After the reaction is completed, the introduction of hydrogen, tantalum pentachloride gas and copper chloride gas is slowly stopped, and argon gas is continuously introduced while maintaining the temperature, and a tantalum coating is obtained after the temperature is lowered.
[0012] Preferably, in step (1), the temperature for the reaction of solid pure tantalum metal with chlorine is 950-1050° C., the chlorine introduction rate is 260-300 ml / min, and the reaction vacuum degree is 10-15 Pa.
[0013] Preferably, in step (1), the argon gas introduction rate is 8000-10000 ml / min.
[0014] Preferably, in step (2), the reaction temperature of cupric chloride is 900-1100°C.
[0015] Preferably, in step (2), the nitrogen introduction rate is 1000-2000 ml / min.
[0016] Preferably, in step (3), the hydrogen introduction rate is 500-600 ml / min, the temperature of the reaction chamber of the CVD equipment is 1000-1150° C., and the reaction time is 3-9 h.
[0017] The present application also provides a tantalum coating obtained by the above-mentioned preparation method.
[0018] Preferably, the tantalum coating is based on tantalum as a matrix, compounded with copper as a composite, and containing trace amounts of tantalum nitride and copper nitride.
[0019] Preferably, the tantalum coating has a thickness of 30-150 μm.
[0020] The present invention has the following outstanding features and beneficial effects: 1. In order to solve the problems of intraoperative infection and postoperative infection in clinical surgery, copper metal is deposited synchronously in the tantalum metal coating. Copper ions have a bactericidal effect, which makes the tantalum metal coating have antibacterial properties. The synergistic effect of tantalum metal and copper metal can solve the infection problem of surgery and improve the effect of human tissue repair. 2. The preparation method of the present invention adopts the technology of synchronous deposition of tantalum and copper metals, which avoids the problem of copper metal covering tantalum metal in multi-layer deposition and the inability to exert the synergistic effect of the two metals, and realizes that both tantalum metal and copper metal can contact human tissues and cells, which helps the tantalum metal coating to regulate cell behavior and promote human bone tissue regeneration. 3. In step (1), tantalum pentachloride is transported under an argon atmosphere, and in step (2), cupric chloride is transported under a nitrogen atmosphere. The composition of the protective atmosphere is controlled in the reaction chamber, and the nitrogen concentration is adjusted to stabilize the tantalum pentachloride gas and the cupric chloride gas, so that a surface coating with tantalum metal as the matrix, composite copper metal, and trace amounts of tantalum nitride and copper nitride is deposited on the surface of the substrate material; the problem of uneven deposition caused by the influence of the gas compounds of the two metals during the simultaneous deposition of the two metal materials is avoided; the bonding force between the coating materials is improved, and the coating is ensured to have mechanical properties compatible with human tissue. DETAILED DESCRIPTION
[0021] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0022] The present invention provides a method for preparing a tantalum coating, comprising the following steps:
[0023] (1) reacting solid pure tantalum metal with chlorine to obtain tantalum pentachloride gas, and introducing the tantalum pentachloride gas into a reaction chamber of a CVD device containing a substrate material through argon transport, wherein the reaction chamber of the CVD device is filled with a high-purity argon atmosphere; wherein the temperature of the reaction of solid pure tantalum metal with chlorine is 950-1050°C, the rate of introduction of chlorine is 260-300 ml / min, the degree of vacuum of the reaction is 10-15 Pa, and the rate of introduction of argon is 8000-10000 ml / min.
[0024] (2) Add cupric chloride powder into a quartz boat and place it in a quartz tube of a tube furnace. Evacuate the quartz tube and introduce nitrogen gas. Heat the tube to obtain cupric chloride gas, and introduce the cupric chloride gas into a reaction chamber of a CVD device. The reaction temperature of the cupric chloride is 900-1100°C and the nitrogen introduction rate is 1000-2000ml / min.
[0025] (3) Hydrogen is introduced into the reaction chamber of the CVD equipment to simultaneously displace tantalum and copper, and tantalum and copper are simultaneously deposited on the surface of the substrate material; wherein the hydrogen introduction rate is 500-600 ml / min, the temperature of the reaction chamber of the CVD equipment is 1000-1150°C, and the reaction time is 3-9 hours.
[0026] (4) After the reaction is completed, the introduction of hydrogen, tantalum pentachloride gas and copper chloride gas is slowly stopped, and argon gas is continuously introduced while maintaining the temperature, and a tantalum coating is obtained after the temperature is lowered.
[0027] The present application also provides a tantalum coating obtained by the above-mentioned preparation method.
[0028] Specifically, the tantalum coating is based on tantalum as a matrix, composited with copper as a composite, and a trace amount of tantalum nitride and copper nitride. The thickness of the tantalum coating is 30-150 μm.
[0029] The present invention is described in detail below in conjunction with specific embodiments, and the beneficial effects of a tantalum coating and a preparation method thereof provided by the present invention are illustrated.
[0030] Example 1
[0031] This embodiment provides a method for preparing a tantalum coating, comprising the following steps:
[0032] (1) Solid pure tantalum metal is reacted with chlorine to obtain tantalum pentachloride gas, which is then introduced into a reaction chamber of a CVD device containing a substrate material through argon transport; the reaction chamber of the CVD device is filled with a high-purity argon atmosphere; the temperature of the reaction of solid pure tantalum metal with chlorine is 950°C, the chlorine introduction rate is 260 ml / min, the reaction vacuum is 10 Pa, and the argon introduction rate is 8000 ml / min.
[0033] (2) Add cupric chloride powder into a quartz boat and place it in a quartz tube of a tube furnace. Evacuate the quartz tube and introduce nitrogen gas. Heat the tube to obtain cupric chloride gas, and introduce the cupric chloride gas into the reaction chamber of the CVD equipment. The reaction temperature of cupric chloride is 900°C and the nitrogen introduction rate is 1000 ml / min.
[0034] (3) Hydrogen is introduced into the reaction chamber of the CVD equipment to simultaneously displace tantalum and copper, which are then deposited on the surface of the substrate material. The hydrogen introduction rate is 500 ml / min, the temperature of the reaction chamber of the CVD equipment is 1000°C, and the reaction time is 3 h.
[0035] (4) After the reaction is completed, the introduction of hydrogen, tantalum pentachloride gas and copper chloride gas is slowly stopped, and argon gas is continuously introduced while maintaining the temperature, and a tantalum coating is obtained after the temperature is lowered.
[0036] The tantalum coating obtained in this embodiment is based on tantalum single substance, composite copper single substance, and trace amounts of tantalum nitride and copper nitride; the thickness of the obtained tantalum coating is 30 μm.
[0037] Example 2
[0038] This embodiment provides a method for preparing a tantalum coating, comprising the following steps:
[0039] (1) Solid pure tantalum metal is reacted with chlorine to obtain tantalum pentachloride gas, and the tantalum pentachloride gas is introduced into a reaction chamber of a CVD device containing a substrate material through argon gas transport; the reaction chamber of the CVD device is filled with a high-purity argon gas atmosphere; the temperature of the reaction of solid pure tantalum metal with chlorine is 980°C, the chlorine gas introduction rate is 270 ml / min, the reaction vacuum is 12 Pa; and the argon gas introduction rate is 8200 ml / min.
[0040] (2) Add cupric chloride powder into a quartz boat and place it in a quartz tube of a tube furnace. Evacuate the quartz tube and introduce nitrogen gas. Heat it to obtain cupric chloride gas, and introduce the cupric chloride gas into the reaction chamber of the CVD equipment. The reaction temperature of cupric chloride is 950°C and the nitrogen introduction rate is 1200 ml / min.
[0041] (3) Hydrogen was introduced into the reaction chamber of the CVD equipment to simultaneously displace tantalum and copper, which were then deposited on the surface of the substrate. The hydrogen introduction rate was 520 ml / min, the temperature of the reaction chamber of the CVD equipment was 1050 °C, and the reaction time was 6 h.
[0042] (4) After the reaction is completed, the introduction of hydrogen, tantalum pentachloride gas and copper chloride gas is slowly stopped, and argon gas is continuously introduced while maintaining the temperature, and a tantalum coating is obtained after the temperature is lowered.
[0043] The tantalum coating obtained in this embodiment is based on tantalum single substance, composite copper single substance, and trace amounts of tantalum nitride and copper nitride; the thickness of the obtained tantalum coating is 90 μm.
[0044] Example 3
[0045] This embodiment provides a method for preparing a tantalum coating, comprising the following steps:
[0046] (1) Solid pure tantalum metal is reacted with chlorine to obtain tantalum pentachloride gas, and the tantalum pentachloride gas is introduced into a reaction chamber of a CVD device containing a substrate material through argon gas transport; the reaction chamber of the CVD device is filled with a high-purity argon gas atmosphere; the temperature of the reaction of solid pure tantalum metal with chlorine is 1050°C, the chlorine gas introduction rate is 300 ml / min, the reaction vacuum is 15 Pa; and the argon gas introduction rate is 10000 ml / min.
[0047] (2) Add cupric chloride powder into a quartz boat and place it in a quartz tube of a tube furnace. Evacuate the quartz tube and introduce nitrogen. Heat it to obtain cupric chloride gas, and introduce the cupric chloride gas into the reaction chamber of the CVD equipment. The reaction temperature of cupric chloride is 1100°C and the nitrogen introduction rate is 2000 ml / min.
[0048] (3) Hydrogen was introduced into the reaction chamber of the CVD equipment to simultaneously displace tantalum and copper, which were then deposited on the surface of the substrate. The hydrogen introduction rate was 600 ml / min, the temperature of the reaction chamber of the CVD equipment was 1150°C, and the reaction time was 9 h.
[0049] (4) After the reaction is completed, the introduction of hydrogen, tantalum pentachloride gas and copper chloride gas is slowly stopped, and argon gas is continuously introduced while maintaining the temperature, and a tantalum coating is obtained after the temperature is lowered.
[0050] The tantalum coating obtained in this embodiment is based on tantalum single substance, composite copper single substance, and trace amounts of tantalum nitride and copper nitride; the obtained tantalum coating has a thickness of 150 μm.
[0051] The tantalum coating and preparation method thereof disclosed in the above embodiment of the present invention have the following advantages: 1. The tantalum coating preparation method provided by the present invention deposits a tantalum metal coating on the surface of a base material by chemical vapor deposition, exerts the high biocompatibility, strong corrosion resistance and excellent osteogenic activity of tantalum metal, improves the bone defect treatment effect of bone implants, and avoids the problems of poor bone bonding and easy loosening of implants caused by insufficient biocompatibility of clinical medical materials. 2. In view of the problems of intraoperative infection and postoperative infection in clinical surgery, copper metal is deposited synchronously in the tantalum metal coating, and copper ions have a bactericidal effect, so that the tantalum metal coating has antibacterial properties. The synergistic enhancement of tantalum metal and copper metal can solve the infection problem of surgery and improve the repair effect of human tissue. 3. The preparation method of the present invention adopts the technology of synchronous deposition of tantalum and copper metals, avoids the problem of copper metal covering tantalum metal in multi-layer deposition and the inability to exert the synergistic effect of the two metals, and realizes that both tantalum metal and copper metal can contact human tissues and cells, which helps the tantalum metal coating to regulate cell behavior and promote human bone tissue regeneration. 4. In step (1), tantalum pentachloride is transported under an argon atmosphere, and in step (2), cupric chloride is transported under a nitrogen atmosphere. The composition of the protective atmosphere is regulated in the reaction chamber, and the nitrogen concentration is adjusted to stabilize the tantalum pentachloride gas and the cupric chloride gas, so that a surface coating with tantalum metal as the matrix, composite copper metal, and trace amounts of tantalum nitride and copper nitride is deposited on the surface of the substrate material; the problem of uneven deposition caused by the influence of the gas compounds of the two metals during the simultaneous deposition of the two metal materials is avoided; the bonding force between the coating materials is improved, and the coating is ensured to have mechanical properties compatible with human tissue.
[0052] The embodiments described above are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application, and should all be included in the protection scope of the present application.
Claims
1. A method for preparing a tantalum coating, characterized in that: The following steps are involved: (1) reacting solid pure tantalum metal with chlorine to obtain tantalum pentachloride gas, and passing the tantalum pentachloride gas into a reaction chamber of a CVD device in which a substrate material is placed through argon gas transport, wherein the reaction chamber of the CVD device is filled with a high-purity argon gas atmosphere; (2) adding cupric chloride powder into a quartz boat and placing the boat in a quartz tube of a tube furnace, evacuating the quartz tube, introducing nitrogen gas, and heating the quartz tube to obtain cupric chloride gas, and introducing the cupric chloride gas into a reaction chamber of the CVD device; (3) introducing hydrogen into the reaction chamber of the CVD device to simultaneously displace tantalum and copper, and the tantalum and copper are simultaneously deposited on the surface of the base material; (4) After the reaction is completed, the introduction of the hydrogen gas, the tantalum pentachloride gas, and the cupric chloride gas is slowly stopped, and the argon gas is continuously introduced while maintaining the temperature, and the tantalum coating is obtained after the temperature is lowered.
2. The method for preparing a tantalum coating according to claim 1, characterized in that: In step (1), the temperature of the reaction between the solid pure tantalum metal and the chlorine gas is 950-1050° C., the chlorine gas introduction rate is 260-300 ml / min, and the reaction vacuum degree is 10-15 Pa.
3. The method for preparing a tantalum coating according to claim 1, characterized in that: In step (1), the argon gas introduction rate is 8000-10000 ml / min.
4. The method for preparing a tantalum coating according to claim 1, characterized in that: In step (2), the reaction temperature of the cupric chloride is 900-1100°C.
5. The method for preparing a tantalum coating according to claim 1, characterized in that: In step (2), the nitrogen introduction rate is 1000-2000 ml / min.
6. The method for preparing a tantalum coating according to claim 1, characterized in that: In step (3), the hydrogen introduction rate is 500-600 ml / min, the temperature of the reaction chamber of the CVD equipment is 1000-1150° C., and the reaction time is 3-9 h.
7. A tantalum coating, characterized in that: Obtained by the preparation method according to any one of claims 1 to 6.
8. A tantalum coating according to claim 7, characterized in that: The tantalum coating takes the tantalum element as a matrix and is compounded with the copper element and trace amounts of tantalum nitride and copper nitride.
9. A tantalum coating according to claim 7, characterized in that: The thickness of the tantalum coating is 30-150 μm.