A light, thin, warm, needle-punched elastic composite material and a preparation method thereof

By combining elastic foam materials with needle-punched cotton fibers, and utilizing the grafting reaction of modified polyvinyl chloride and modified silica aerogel, a thin and warm needle-punched composite material with excellent antibacterial and flame retardant properties is formed. It solves the limitations of existing materials in terms of antibacterial performance and flame retardant performance, and achieves thinness, lightness, thermal insulation and improved comfort of the material.

CN118163441BActive Publication Date: 2024-10-01SYCORETC CAS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410298287.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-15
Publication Date
2024-10-01
Estimated Expiration
2044-03-15

AI Technical Summary

Technical Problem

Existing thermal clothing materials have limitations in improving antibacterial performance and flame retardant performance. In particular, the loss of copper ions leads to poor durability of antibacterial performance, and their thickness affects comfort and appearance.

Method used

The elastic foam material is combined with needle-punched cotton fiber, blended through nitrile rubber, polyamide, modified polyvinyl chloride and modified silica airgel, and the antibacterial and flame retardant molecules in the modifier are grafted Reaction to form a thin, warm and needle-punched elastic composite material with good antibacterial and flame retardant properties.

Benefits of technology

The composite material is light and thin, has good resilience, has thermal insulation properties, and has excellent antibacterial, mildew-proof, and flame-retardant properties, making it suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118163441B_ABST
    Figure CN118163441B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of composite materials, and in particular, relates to a thin and light warm needle-punched elastic composite material and a preparation method thereof. The composite material is formed by compounding an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located on one side surface of the elastic foam material or on both sides of the elastic foam material or in the middle of two layers of elastic foam material; the elastic foam material is a blended foam material of nitrile rubber, polyamide, modified polyvinyl chloride, and modified silica aerogel; the present invention first prepares an elastic foam material, and then compound the elastic foam material and needle-punched cotton fibers through needle-punching to obtain a composite material; the thin and light warm needle-punched elastic composite material prepared by the present invention using elastic foam material and needle-punched cotton fibers is thin and light, has good resilience, thermal insulation and mechanical properties, especially excellent antibacterial and mildew-proof and flame-retardant properties, and has a wide range of applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and particularly relates to a light, thin, warm-keeping, needle-punched elastic composite material and a preparation method thereof. Background Art

[0002] As a necessity of life, thermal clothing plays a very important role in regulating human body temperature and maintaining normal human functions. Traditional thermal clothing mostly uses natural fibers. By increasing the thickness of clothing or increasing the filling density to improve the thermal insulation effect, but too much thickness will cause the clothing to be bulky, affecting human activities and the beauty of clothing. With the continuous improvement of living standards, people have put forward more requirements on the performance of thermal clothing. In addition to the requirements of cold protection and warmth preservation, they also emphasize comfort and beauty. More and more thermal insulation materials are also used in the field of thermal insulation clothing. At present, the most widely used thermal insulation materials are porous foam materials and silica aerogels. Among them, porous foam materials have lower thermal conductivity and higher porosity, which can effectively block heat transfer and absorb moisture in the air, so as to have good thermal insulation performance. Silica aerogel is an open-pore nanomaterial with a three-dimensional skeleton structure, which has excellent characteristics such as low density, low thermal conductivity, high porosity, and high specific surface area. It has good thermal insulation effect and long service life. Multifunctional composite materials based on porous foam materials and silica aerogels have also become a research hotspot in recent years.

[0003] The patent with application number 202211527426.3 discloses a method for preparing an antibacterial hydrophobic silica aerogel composite material. Tetraethyl orthosilicate is used as a silicon source, and deionized water and anhydrous ethanol are added to prepare silica gel. After five subsequent treatments at a certain temperature, including silica skeleton aging, solvent exchange, gel surface hydrophobic modification, atmospheric pressure blower drying and copper ion loading, an antibacterial hydrophobic silica aerogel composite material is obtained, in which copper ions with antibacterial effect are loaded onto the aerogel surface through coordination bonds. The coordination bond force formed is not strong enough, which easily causes the loss of copper ions, resulting in poor durability of the antibacterial performance of the composite material. The patent with application number 202211569692.2 discloses a modified polymer aerogel composite material and a preparation method thereof. Tetraethoxysilane and 3-aminopropyltriethoxysilane are used as composite silicon precursors and modified with decanoic acid to obtain modified silica aerogel, and further a foamable material and modified silica aerogel are blended to obtain a modified polymer aerogel composite material. The prepared composite material has low density, good thermal insulation and flame retardant effects, excellent mechanical properties, and high comfort, but its comprehensive performance still has room for improvement, and its application field has certain limitations. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a light, thin, warm needle-punched elastic composite material and a preparation method thereof. The light, thin, warm needle-punched elastic composite material prepared by elastic foam material and needle-punched cotton fiber is light, has good resilience, thermal insulation and mechanical properties, especially antibacterial and mildew-proof and flame retardant properties, and has a wide range of applications.

[0005] The technical solution adopted by the present invention to solve the above problems is:

[0006] A light, thin, warm-keeping needle-punched elastic composite material, wherein the composite material is formed by compounding an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located on one side surface of the elastic foam material or on both sides of the elastic foam material or in the middle of two layers of elastic foam material;

[0007] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0008] The present invention provides a method for preparing a light, thin, warm, needle-punched elastic composite material, which comprises the following steps in parts by weight:

[0009] A1. After uniformly mixing 40-50 parts of polyamide, 30-40 parts of modified polyvinyl chloride, 10-15 parts of plasticizer and 5-8 parts of heat stabilizer, add them into an internal mixer, heat them to 120-130°C, mix them for 5-10 minutes, add 60-70 parts of nitrile rubber, 2-3 parts of antioxidant and 5-10 parts of filler, continue to heat them to 150-160°C, mix them for 15-20 minutes to obtain a masterbatch;

[0010] A2, adding 10-15 parts of foaming agent, 6-10 parts of vulcanizing agent, 3-5 parts of vulcanization accelerator and 30-35 parts of modified silica aerogel to the masterbatch, cooling to 90-100°C, mixing for 3-5 minutes to obtain a rubber mix; putting the rubber mix into an extruder, extruding it into a desired shape, and then putting it into a molding machine for curing, and rapidly cooling it at a speed greater than 4°C / s to obtain an elastic foam material;

[0011] A3. Place needle-punched cotton fibers on one side surface of the elastic foam material or on both side surfaces of the elastic foam material or in the middle of two layers of elastic foam material, and compound them by needle-punching to obtain a composite material.

[0012] Furthermore, the curing process in step A2 is as follows: the first curing pressure is 10-15MPa, the temperature is 130-150°C, and the time is 15-20min; the second curing pressure is 15-20MPa, the temperature is 170-180°C, and the time is 10-15min.

[0013] The present invention also provides an application of the above-mentioned thin and light warm needle-punched elastic composite material, and the composite material is used in clothing, shoes and hats, cold chain packaging, construction, and aerospace fields.

[0014] The preparation method of modified polyvinyl chloride is as follows: polyvinyl chloride, a modifier and triethylamine are added to N,N-dimethylacetamide, the temperature is raised to 80-90°C, and the mixture is stirred for reaction for 8-10 hours. After the reaction is completed, the mixture is naturally cooled to room temperature, glycerol is added until no precipitate is precipitated, the mixture is filtered, the precipitate is washed with water for 3 times, and the modified polyvinyl chloride is obtained after drying.

[0015] Furthermore, the mass ratio of the polyvinyl chloride, the modifier and the triethylamine is 1:0.6-0.8:0.1-0.2.

[0016] The preparation method of modified silica aerogel is:

[0017] S1, adding methyltrimethoxysilane and 3-aminopropyltrimethoxysilane to a mixed solvent, stirring and mixing evenly, adding 0.5-1 mol / L sulfuric acid to adjust the pH value of the solvent to 2-3 for hydrolysis, and then adding ammonia water to adjust the pH value of the solvent to 10-11 for condensation to obtain a wet gel;

[0018] S2, adding modified quaternary ammonium salt and N,N'-carbonyldiimidazole to acetonitrile and water, heating to 30-40°C, stirring for 5-6h, removing acetonitrile to obtain a mixed solution, adding the mixed solution to the wet gel obtained in step S1, continuing to heat to 60-70°C, reacting for 6-8h to obtain a modified wet gel, washing with acetone and then supercritical drying to obtain a modified silica aerogel;

[0019] Furthermore, in step S1, the mass ratio of methyltrimethoxysilane, 3-aminopropyltrimethoxysilane and the mixed solvent is 1:0.8-1:4-5; and the mixed solvent is ethanol and water in a mass ratio of 1:0.1-0.2.

[0020] Furthermore, the amount of the modified quaternary ammonium salt in step S2 is the same as the molar amount of 3-aminopropyltrimethoxysilane in step S1; and the molar ratio of the modified quaternary ammonium salt to N,N'-carbonyldiimidazole is 1:1-1.1.

[0021] The preparation method of the modifier is:

[0022] (1) Add diethylenetriamine to chloroform, raise the temperature to 40-50°C, slowly add epichlorohydrin, continue the reaction for 3-4 hours, and concentrate under reduced pressure to obtain chlorinated diethylenetriamine, the chemical structure of which is:

[0023] ;

[0024] (2) Add diethylenetriamine chloride and dodecyldimethylamine to ethanol, heat to 80°C, and reflux for 10-12 hours to obtain a modified quaternary ammonium salt with the chemical formula:

[0025] ;

[0026] (3) Add the modified quaternary ammonium salt and triethylamine to a mixed solvent of anhydrous ether and acetonitrile, add diethylphosphite chloride dropwise under ice bath conditions, continue the reaction for 2-3 hours, and obtain a modifier having the chemical structure:

[0027] .

[0028] Furthermore, the molar ratio of diethylenetriamine to epichlorohydrin in step (1) is 1:2-2.1; the molar ratio of diethylenetriamine chloride to dodecyldimethyl tertiary amine in step (2) is 1:1-1.1; and the molar ratio of the modifier quaternary ammonium salt, diethylphosphite chloride, and triethylamine in step (3) is 1:1-1.1:1.5-2.0.

[0029] The present invention has the following beneficial effects:

[0030] The molecular structure of the modifier prepared by the present invention contains a diquaternary ammonium salt with antibacterial effect and a phosphorus element with flame retardant effect. The -NH in the modifier reacts with the C-Cl bond in the polyvinyl chloride to form a grafting reaction, and the modifier is successfully grafted onto the polyvinyl chloride molecular chain to obtain a modified polyvinyl chloride with antibacterial and flame retardant effect. The molecular structure of the modified quaternary ammonium salt prepared by the present invention also contains a diquaternary ammonium salt with antibacterial effect. The -OH in the modified quaternary ammonium salt reacts with the -NH2 on the surface of the wet gel under the action of N,N'-carbonyldiimidazole to form a condensation reaction, and the modified quaternary ammonium salt is successfully grafted onto the silica aerogel to obtain a modified silica aerogel with antibacterial effect. The present invention further In the first step, modified polyvinyl chloride and modified silica aerogel are used to prepare composite materials. On the one hand, modified polyvinyl chloride and modified silica aerogel can work together to improve the antibacterial properties of the composite materials. On the other hand, the two can also synergize with other flame retardant components to significantly improve the flame retardant properties of the composite materials. In addition, since similar organic molecules (long-chain quaternary ammonium salts with good dispersibility) are grafted on the surfaces of modified polyvinyl chloride and modified silica aerogel, the two have good compatibility and good dispersibility in the mixed system. During the mixing process, the components can be mixed more fully and the bonding force is stronger, thereby improving the comprehensive performance of the composite materials.

[0031] The light and thin warm-keeping needle-punched elastic composite material prepared by the present invention using elastic foam material and needle-punched cotton fiber is light and thin, has good resilience, thermal insulation and mechanical properties, especially excellent antibacterial and mildew-proof and flame-retardant properties, and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagrams of three structures of composite materials; among them, 1 is elastic foam material and 2 is needle-punched cotton fiber.

[0033] Figure 2 This is a physical picture of the composite material prepared by the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0035] The raw materials used in the following examples are all common commercial products. Among them, polyvinyl chloride (S-60) CAS No. 9002-86-2; methyltrimethoxysilane CAS No. 1185-55-3; 3-aminopropyltrimethoxysilane CAS No. 13822-56-5; sulfuric acid CAS No. 7664-93-9; ammonia CAS No. 1336-21-6; N,N'-carbonyldiimidazole CAS No. 530-62-1; diethylenetriamine CAS No. 111-40-0; epichlorohydrin CAS No. 106-89-8; dodecyl dimethyl tert-butyl ester Amine CAS No. 112-18-5; diethylphosphite chloride CAS No. 589-57-1; triethylamine CAS No. 121-44-8; chloroform CAS No. 67-66-3; ether CAS No. 60-29-7; acetonitrile CAS No. 75-05-8; N,N-dimethylacetamide CAS No. 127-19-5; glycerol CAS No. 56-81-5; dichloromethane CAS No. 75-09-2; ethanol CAS No. 64-17-5; acetone CAS No. 67-64-1.

[0036] The needle-punched cotton fiber used in the present invention is a flake directly obtained by punching polyester fiber, polyester and polypropylene with needles. The needle-punched cotton is also called needle-punched non-woven fabric, which is a kind of dry non-woven fabric. It is a non-woven fabric made of polyester fiber, polyester and polypropylene by a needle-punching machine. The needle-punched cotton has the advantages of flame retardancy, heat insulation, sound absorption and sound insulation. The needle-punched cotton is usually used as a filling material and is widely used in clothing, electric heating plates, cushions, household items and other fields.

[0037] In the preparation method of the composite material provided by the present invention, the plasticizer is dioctyl phthalate; the heat stabilizer is a calcium-zinc composite stabilizer; the antioxidant is N-phenyl-N'-cyclohexyl-p-phenylenediamine; the filler is white carbon black; the foaming agent is azodicarbonamide; the vulcanizing agent is sulfur; and the vulcanization accelerator is vulcanization accelerator D.

[0038] Example 1

[0039] A light, thin, warm, needle-punched elastic composite material, the composite material is made of an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located between two layers of elastic foam materials;

[0040] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0041] The present invention provides a method for preparing a light, thin, warm, needle-punched elastic composite material, which comprises the following steps in parts by weight:

[0042] A1. After mixing 50 parts of polyamide, 40 parts of modified polyvinyl chloride, 15 parts of plasticizer and 8 parts of heat stabilizer, add them into an internal mixer, heat them to 130°C, mix them for 5 minutes, add 70 parts of nitrile rubber, 3 parts of antioxidant and 10 parts of filler, continue to heat them to 160°C, mix them for 15 minutes to obtain a masterbatch;

[0043] A2. Add 15 parts of foaming agent, 10 parts of vulcanizing agent, 5 parts of vulcanization accelerator and 35 parts of modified silica aerogel to the masterbatch, cool to 100°C, and mix for 3 minutes to obtain a rubber mix; put the rubber mix into an extruder, extrude into a desired shape, and then put it into a molding machine for curing, and quickly cool at a speed of more than 4°C / s to obtain an elastic foam material; wherein the curing process is as follows: the first curing pressure is 15MPa, the temperature is 130°C, and the time is 20min; the second curing pressure is 20MPa, the temperature is 170°C, and the time is 15min;

[0044] A3. Place the needle-punched cotton fiber between two layers of elastic foam material and compound them by needle-punching to obtain a composite material.

[0045] The preparation method of modified polyvinyl chloride is as follows: polyvinyl chloride, a modifier and triethylamine are added to N,N-dimethylacetamide, the temperature is raised to 90°C, and the reaction is stirred for 10 hours. After the reaction is completed, the temperature is naturally lowered to room temperature, glycerol is added until no precipitate is precipitated, and the precipitate is filtered, and the precipitate is washed with water for 3 times, and the modified polyvinyl chloride is obtained after drying; wherein the mass ratio of polyvinyl chloride, the modifier and the triethylamine is 1:0.8:0.2; and the amount of N,N-dimethylacetamide used is 10 times the mass of polyvinyl chloride.

[0046] The preparation method of modified silica aerogel is:

[0047] S1, adding methyltrimethoxysilane and 3-aminopropyltrimethoxysilane to a mixed solvent, stirring and mixing evenly, adding 1 mol / L sulfuric acid to adjust the pH value of the solvent to 3 for hydrolysis, and then adding ammonia water to adjust the pH value of the solvent to 10 for condensation to obtain a wet gel; wherein the mass ratio of methyltrimethoxysilane, 3-aminopropyltrimethoxysilane and the mixed solvent is 1:1:5; the mixed solvent is ethanol and water in a mass ratio of 1:0.2;

[0048] S2, adding modified quaternary ammonium salt and N,N'-carbonyldiimidazole to acetonitrile and water, heating to 40°C, stirring for 5 hours, removing acetonitrile to obtain a mixed solution, adding the mixed solution to the wet gel obtained in step S1, continuing to heat to 70°C, reacting for 6 hours to obtain a modified wet gel, washing with acetone and then supercritical drying to obtain a modified silica aerogel; wherein the amount of the modified quaternary ammonium salt is the same as the molar amount of 3-aminopropyltrimethoxysilane in step S1; the molar ratio of the modified quaternary ammonium salt and N,N'-carbonyldiimidazole is 1:1; the mass ratio of acetonitrile to water is 2:1, and the amount of water is twice the mass of the modified quaternary ammonium salt.

[0049] The preparation method of the modifier is:

[0050] (1) Add 21.0 g of diethylenetriamine to 1000 mL of chloroform, raise the temperature to 50°C, slowly drop 37.7 g of epichlorohydrin, continue the reaction for 4 hours, and after the reaction is completed, naturally cool to room temperature, remove chloroform, add 800 mL of water and 800 mL of dichloromethane for extraction, collect the organic phase, and concentrate under reduced pressure to obtain 46.7 g of chlorinated diethylenetriamine; the molar ratio of diethylenetriamine to epichlorohydrin is 1:2; the reaction process is:

[0051] ;

[0052] Diethylenetriamine chloride: ESI (m / z): 289.2 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 5.37 (s, 2H), 3.86-3.88 (m, 2H), 3.71 (s, 2H), 3.63 -3.65 (m, 2H), 3.38-3.40 (m, 2H), 2.74-2.77 (m, 6H), 2.53-2.56 (m, 6H), 1.5 (s, 1H).

[0053] (2) 45.0 g of diethylenetriamine chloride and 33.3 g of dodecyldimethylamine were added to 400 mL of ethanol, the temperature was raised to 80°C, and the reaction was refluxed for 12 h. After the reaction was completed, the temperature was naturally cooled to room temperature, the ethanol was removed, 500 mL of water and 500 mL of dichloromethane were added for extraction, the aqueous phase was collected, and the phase was concentrated under reduced pressure to obtain 89.5 g of modified quaternary ammonium salt. The molar ratio of diethylenetriamine chloride to dodecyldimethylamine was 1:1. The reaction process was as follows:

[0054] ;

[0055] Modified quaternary ammonium salt: ESI (m / z): 716.0 [M+H] + , 1 H-NMR (600MHz, DMSO-d6, δppm): 5.37 (s, 2H), 4.17-4.20 (m, 2H), 3.70 (s, 2H), 3.50-3.53 (m, 2H), 3.30 (s, 12H), 3.22-3.2 5 (m, 6H), 2.78-2.81 (m, 6H), 2.52-2.55 (m, 6H), 1.71-1.74 (m, 4H), 1.5 (s, 1H), 1.26-1.29 (m, 36H), 0.88 (t, J=7.4Hz, 6H).

[0056] (3) 71.5.0 g of modified quaternary ammonium salt and 15.2 g of triethylamine were added to a mixed solvent of 600 mL of anhydrous ether and acetonitrile (volume ratio of 2:1), and 15.7 g of diethylphosphite chloride was added dropwise under ice bath conditions. After the addition was completed, the reaction was continued for 3 h. After the reaction was completed, the mixed solvent was removed, 600 mL of water and 600 mL of dichloromethane were added for extraction, the aqueous phase was collected, and the molar ratio of the modifier quaternary ammonium salt, diethylphosphite chloride, and triethylamine was 1:1:1.5; the reaction process was:

[0057] ;

[0058] Modifier: ESI (m / z): 478.6 [M / 2+H] + , 1H-NMR (600MHz, DMSO-d6, δppm): 4.20-4.22 (m, 2H), 3.85-3.88 (m, 8H), 3.70 (s, 2H), 3.51-3.53 (m, 2H), 3.30 (s, 12H), 3.23-3 .26 (m, 6H), 2.76-2.79 (m, 6H), 2.53-2.56 (m, 6H), 1.70-1.72 (m, 4H), 1.5 (s, 1H), 1.25-1.29 (m, 48H), 0.88 (t, J=7.4Hz, 6H).

[0059] Example 2

[0060] A light, thin, warm, needle-punched elastic composite material, the composite material is made of an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located between two layers of elastic foam materials;

[0061] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0062] The present invention provides a method for preparing a light, thin, warm, needle-punched elastic composite material, which comprises the following steps in parts by weight:

[0063] A1. After uniformly mixing 40 parts of polyamide, 30 parts of modified polyvinyl chloride, 10 parts of plasticizer and 5 parts of heat stabilizer, add them into an internal mixer, heat them to 120°C, mix them for 10 minutes, add 60 parts of nitrile rubber, 2 parts of antioxidant and 5 parts of filler, continue to heat them to 150°C, mix them for 20 minutes to obtain a masterbatch;

[0064] A2. Add 10 parts of foaming agent, 6 parts of vulcanizing agent, 3 parts of vulcanization accelerator and 30 parts of modified silica aerogel to the masterbatch, cool to 90°C, and mix for 5 minutes to obtain a rubber mix; put the rubber mix into an extruder, extrude into a desired shape, and then put it into a molding machine for curing, and quickly cool at a speed of more than 4°C / s to obtain an elastic foam material; wherein the curing process is as follows: the first curing pressure is 10MPa, the temperature is 150°C, and the time is 15min; the second curing pressure is 15MPa, the temperature is 180°C, and the time is 10min;

[0065] A3. Place the needle-punched cotton fiber between two layers of elastic foam material and compound them by needle-punching to obtain a composite material.

[0066] The preparation method of modified polyvinyl chloride is as follows: polyvinyl chloride, a modifier and triethylamine are added to N,N-dimethylacetamide, the temperature is raised to 80°C, and the reaction is stirred for 8 hours. After the reaction is completed, the temperature is naturally lowered to room temperature, glycerol is added until no precipitate is precipitated, and the precipitate is filtered, and the precipitate is washed with water for 3 times, and the modified polyvinyl chloride is obtained after drying; wherein the mass ratio of polyvinyl chloride, the modifier and the triethylamine is 1:0.6:0.1; and the amount of N,N-dimethylacetamide used is 10 times the mass of polyvinyl chloride.

[0067] The preparation method of modified silica aerogel is:

[0068] S1, adding methyltrimethoxysilane and 3-aminopropyltrimethoxysilane to a mixed solvent, stirring and mixing evenly, adding 0.5 mol / L sulfuric acid to adjust the pH value of the solvent to 2 for hydrolysis, and then adding ammonia water to adjust the pH value of the solvent to 10.5 for condensation to obtain a wet gel; wherein the mass ratio of methyltrimethoxysilane, 3-aminopropyltrimethoxysilane and the mixed solvent is 1:0.8:4; the mixed solvent is ethanol and water in a mass ratio of 1:0.1;

[0069] S2, adding modified quaternary ammonium salt and N,N'-carbonyldiimidazole to acetonitrile and water, heating to 30°C, stirring for 6h, removing acetonitrile to obtain a mixed solution, adding the mixed solution to the wet gel obtained in step S1, continuing to heat to 60°C, reacting for 8h to obtain a modified wet gel, washing with acetone and then supercritical drying to obtain a modified silica aerogel; wherein the amount of the modified quaternary ammonium salt is the same as the molar amount of 3-aminopropyltrimethoxysilane in step S1; the molar ratio of the modified quaternary ammonium salt to N,N'-carbonyldiimidazole is 1:1.1; the mass ratio of acetonitrile to water is 2:1, and the amount of water is twice the mass of the modified quaternary ammonium salt.

[0070] The preparation method of the modifier is the same as that of Example 1.

[0071] Example 3

[0072] A light, thin, warm, needle-punched elastic composite material, the composite material is made of an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located between two layers of elastic foam materials;

[0073] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0074] The present invention provides a method for preparing a light, thin, warm and elastic needle-punched composite material, which comprises the following steps in parts by weight:

[0075] A1. After mixing 45 parts of polyamide, 35 parts of modified polyvinyl chloride, 12 parts of plasticizer and 7 parts of heat stabilizer, add them into an internal mixer, heat them to 125°C, mix them for 8 minutes, add 65 parts of nitrile rubber, 2 parts of antioxidant and 8 parts of filler, continue to heat them to 155°C, mix them for 18 minutes to obtain a masterbatch;

[0076] A2. Add 12 parts of foaming agent, 7 parts of vulcanizing agent, 4 parts of vulcanization accelerator and 33 parts of modified silica aerogel to the masterbatch, cool to 95°C, and mix for 4 minutes to obtain a rubber mix; put the rubber mix into an extruder, extrude into a desired shape, and then put it into a molding machine for curing, and quickly cool at a speed of more than 4°C / s to obtain an elastic foam material; wherein the curing process is as follows: the first curing pressure is 13MPa, the temperature is 140°C, and the time is 15min; the second curing pressure is 18MPa, the temperature is 175°C, and the time is 12min;

[0077] A3. Place the needle-punched cotton fiber between two layers of elastic foam material and compound them by needle-punching to obtain a composite material.

[0078] The preparation method of modified polyvinyl chloride is as follows: polyvinyl chloride, a modifier and triethylamine are added to N,N-dimethylacetamide, the temperature is raised to 85°C, and the reaction is stirred for 8 hours. After the reaction is completed, the temperature is naturally lowered to room temperature, glycerol is added until no precipitate is precipitated, and the precipitate is filtered, and the precipitate is washed with water for 3 times, and the modified polyvinyl chloride is obtained after drying; wherein the mass ratio of polyvinyl chloride, the modifier and the triethylamine is 1:0.7:0.2; and the amount of N,N-dimethylacetamide used is 10 times the mass of polyvinyl chloride.

[0079] The preparation method of modified silica aerogel is:

[0080] S1, adding methyltrimethoxysilane and 3-aminopropyltrimethoxysilane to a mixed solvent, stirring and mixing evenly, adding 1 mol / L sulfuric acid to adjust the pH value of the solvent to 2.5 for hydrolysis, and then adding ammonia water to adjust the pH value of the solvent to 11 for condensation to obtain a wet gel; wherein the mass ratio of methyltrimethoxysilane, 3-aminopropyltrimethoxysilane and the mixed solvent is 1:0.9:5; the mixed solvent is ethanol and water in a mass ratio of 1:0.2;

[0081] S2, adding modified quaternary ammonium salt and N,N'-carbonyldiimidazole to acetonitrile and water, heating to 35°C, stirring for 6h, removing acetonitrile to obtain a mixed solution, adding the mixed solution to the wet gel obtained in step S1, continuing to heat to 65°C, reacting for 7h to obtain a modified wet gel, washing with acetone and then supercritical drying to obtain a modified silica aerogel; wherein the amount of the modified quaternary ammonium salt is the same as the molar amount of 3-aminopropyltrimethoxysilane in step S1; the molar ratio of the modified quaternary ammonium salt and N,N'-carbonyldiimidazole is 1:1; the mass ratio of acetonitrile to water is 2:1, and the amount of water is twice the mass of the modified quaternary ammonium salt.

[0082] The preparation method of the modifier is the same as that of Example 1.

[0083] Comparative Example 1

[0084] A light, thin, warm, needle-punched elastic composite material, the composite material is made of an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located between two layers of elastic foam materials;

[0085] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0086] The present invention provides a method for preparing a light, thin, warm and elastic needle-punched composite material, which comprises the following steps in parts by weight:

[0087] A1. After 50 parts of polyamide, 40 parts of polyvinyl chloride, 15 parts of plasticizer and 8 parts of heat stabilizer are mixed evenly, the mixture is added into an internal mixer, the mixture is heated to 130°C and mixed for 5 minutes, 70 parts of nitrile rubber, 3 parts of antioxidant and 10 parts of filler are added, the mixture is heated to 160°C and mixed for 15 minutes to obtain a masterbatch;

[0088] A2. Add 15 parts of foaming agent, 10 parts of vulcanizing agent, 5 parts of vulcanization accelerator and 35 parts of modified silica aerogel to the masterbatch, cool to 100°C, and mix for 3 minutes to obtain a rubber mix; put the rubber mix into an extruder, extrude into a desired shape, and then put it into a molding machine for curing, and quickly cool at a speed of more than 4°C / s to obtain an elastic foam material; wherein the curing process is as follows: the first curing pressure is 15MPa, the temperature is 130°C, and the time is 20min; the second curing pressure is 20MPa, the temperature is 170°C, and the time is 15min;

[0089] A3. Place the needle-punched cotton fiber between two layers of elastic foam material and compound them by needle-punching to obtain a composite material.

[0090] The preparation method of modified silica aerogel is the same as that in Example 1.

[0091] Comparative Example 2

[0092] A light, thin, warm, needle-punched elastic composite material, the composite material is made of an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located between two layers of elastic foam materials;

[0093] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0094] The present invention provides a method for preparing a light, thin, warm and elastic needle-punched composite material, which comprises the following steps in parts by weight:

[0095] A1. After mixing 50 parts of polyamide, 40 parts of modified polyvinyl chloride, 15 parts of plasticizer and 8 parts of heat stabilizer, add them into an internal mixer, heat them to 130°C, mix them for 5 minutes, add 70 parts of nitrile rubber, 3 parts of antioxidant and 10 parts of filler, continue to heat them to 160°C, mix them for 15 minutes to obtain a masterbatch;

[0096] A2. Add 15 parts of foaming agent, 10 parts of vulcanizing agent, 5 parts of vulcanization accelerator and 35 parts of silica aerogel to the masterbatch, cool to 100°C, and mix for 3 minutes to obtain a rubber mix; put the rubber mix into an extruder, extrude into a desired shape, and then put it into a molding machine for curing, and quickly cool at a speed greater than 4°C / s to obtain an elastic foam material; wherein the curing process is as follows: the first curing pressure is 15MPa, the temperature is 130°C, and the time is 20min; the second curing pressure is 20MPa, the temperature is 170°C, and the time is 15min;

[0097] A3. Place the needle-punched cotton fiber between two layers of elastic foam material and compound them by needle-punching to obtain a composite material.

[0098] The preparation method of modified polyvinyl chloride is the same as that in Example 1.

[0099] The preparation method of silica aerogel is:

[0100] S1, the same as step S1 in Example 1;

[0101] S2. Wash the wet gel obtained in step S1 with acetone and then dry it by supercritical drying to obtain silica aerogel.

[0102] Comparative Example 3

[0103] A light, thin, warm, needle-punched elastic composite material, the composite material is made of an elastic foam material and needle-punched cotton fibers through needle-punching; the needle-punched cotton fibers are located between two layers of elastic foam materials;

[0104] The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel;

[0105] The present invention provides a method for preparing a light, thin, warm, needle-punched elastic composite material, which comprises the following steps in parts by weight:

[0106] A1. After 50 parts of polyamide, 40 parts of polyvinyl chloride, 15 parts of plasticizer and 8 parts of heat stabilizer are mixed evenly, the mixture is added into an internal mixer, the mixture is heated to 130°C and mixed for 5 minutes, 70 parts of nitrile rubber, 3 parts of antioxidant and 10 parts of filler are added, the mixture is heated to 160°C and mixed for 15 minutes to obtain a masterbatch;

[0107] A2. Add 15 parts of foaming agent, 10 parts of vulcanizing agent, 5 parts of vulcanization accelerator and 35 parts of silica aerogel to the masterbatch, cool to 100°C, and mix for 3 minutes to obtain a rubber mix; put the rubber mix into an extruder, extrude into a desired shape, and then put it into a molding machine for curing, and quickly cool at a speed greater than 4°C / s to obtain an elastic foam material; wherein the curing process is as follows: the first curing pressure is 15MPa, the temperature is 130°C, and the time is 20min; the second curing pressure is 20MPa, the temperature is 170°C, and the time is 15min;

[0108] A3. Place the needle-punched cotton fiber between two layers of elastic foam material and compound them by needle-punching to obtain a composite material.

[0109] The preparation method of silica aerogel is the same as that of Comparative Example 2.

[0110] 1. Basic performance test of composite materials

[0111] The basic performance tests of composite materials include density, thermal conductivity, resilience and mechanical properties. The thermal conductivity is tested by Hot Disk test, and the mechanical properties (tensile strength, compressive strength) are tested by CMT6104 universal testing machine. Rebound: compress the sample to 10% of the original height, remove the compression, and then compress it to 10% of the original height, remove the compression, and repeat this 50 times. Calculate the ratio of the height of the sample after removing the compression to the original height. The higher the ratio, the better the material's resilience. The test results are shown in Table 1.

[0112] Table 1 Basic performance test results of composite materials

[0113]

[0114] From the analysis of the test results in Table 1, it can be seen that the composite materials prepared by Examples 1-3 of the present invention are light and thin, have good thermal insulation performance, and also have good resilience and mechanical properties; compared with Comparative Examples 1-3, Example 1 of the present invention uses modified polyvinyl chloride and modified silica aerogel as raw materials for preparing a light and warm needle-punched elastic composite material. The surfaces of modified polyvinyl chloride and modified silica aerogel are grafted with similar organic molecules (containing long-chain quaternary ammonium salts with good dispersing effects). The two have good compatibility and good dispersibility in the mixed system. During the mixing process, the components can be mixed more fully and the bonding force is stronger, thereby improving the comprehensive performance of the composite material.

[0115] 2. Antibacterial and flame retardant properties test of composite materials

[0116] The antibacterial performance test of the composite material refers to the GB / T20944.2-2007 standard, and the flame retardant performance test refers to the GB / T8624-2012 standard. The test results are shown in Table 2.

[0117] Table 2 Antibacterial and flame retardant test results of composite materials

[0118]

[0119] From the analysis of the test results in Table 2, it can be seen that the antibacterial rates of the composite materials of Examples 1-3 of the present invention against Staphylococcus aureus, Escherichia coli, Aspergillus niger, and Trichoderma are all above 95%, and the combustion grade reaches A1, indicating that the composite materials prepared by the present invention have excellent antibacterial and flame retardant properties; compared with Comparative Examples 1-3, the raw materials used in Example 1 of the present invention are modified polyvinyl chloride and modified silica aerogel, and the surfaces of the modified polyvinyl chloride and the modified silica aerogel are grafted with organic molecules containing phosphorus elements with flame retardant effects and diquaternary ammonium salts with antibacterial effects. On the one hand, the two can work together to improve the antibacterial properties of the composite material, and on the other hand, the two can also synergize with other flame retardant components to significantly improve the flame retardant properties of the composite material.

[0120] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also includes other elements that are not explicitly listed, or also includes elements inherent to such process, method, article or device; although the embodiments of the present application have been shown and described, it can be understood by those of ordinary skill in the art that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present application, and the scope of the present application is defined by the appended claims and their equivalents.

Claims

1. A thin and light warm needle-punched elastic composite material, characterized in that: The composite material is formed by compounding an elastic foam material and needle-punched cotton fibers through needle punching; the needle-punched cotton fibers are located on one side surface of the elastic foam material or on both sides of the elastic foam material or in the middle of two layers of elastic foam material; The elastic foaming material is a blended foaming material of nitrile rubber, polyamide, modified polyvinyl chloride and modified silica aerogel; The preparation method of the modified polyvinyl chloride is as follows: polyvinyl chloride, a modifier and triethylamine are added to N,N-dimethylacetamide, the temperature is raised to 80-90° C., and the reaction is stirred for 8-10 hours to obtain the modified polyvinyl chloride; the chemical structural formula of the modifier is: ; The preparation method of the modified silica aerogel is: S1, adding methyltrimethoxysilane and 3-aminopropyltrimethoxysilane to a mixed solvent, stirring and mixing evenly, adding 0.5-1 mol / L sulfuric acid to adjust the pH value of the solvent to 2-3 for hydrolysis, and then adding ammonia water to adjust the pH value of the solvent to 10-11 for condensation to obtain a wet gel; S2, adding modified quaternary ammonium salt and N,N'-carbonyldiimidazole to acetonitrile and water, heating to 30-40°C, stirring for 5-6h, removing acetonitrile to obtain a mixed solution, adding the mixed solution to the wet gel obtained in step S1, continuing to heat to 60-70°C, reacting for 6-8h to obtain a modified wet gel, washing with acetone and then supercritical drying to obtain a modified silica aerogel; the chemical structural formula of the modified quaternary ammonium salt is: 。 2. The thin and light warm needle-punched elastic composite material according to claim 1, characterized in that: The preparation method of the modifier is: (1) Add diethylenetriamine to chloroform, raise the temperature to 40-50°C, slowly add epichlorohydrin, continue the reaction for 3-4 hours, and concentrate under reduced pressure to obtain chlorinated diethylenetriamine, the chemical structure of which is: ; (2) adding diethylenetriamine chloride and dodecyldimethyl tertiary amine to ethanol, heating to 80°C, and reflux reaction for 10-12 hours to obtain a modified quaternary ammonium salt; (3) Add the modified quaternary ammonium salt and triethylamine to a mixed solvent of anhydrous ether and acetonitrile, and add diethylphosphite chloride dropwise under ice bath conditions. After the addition is complete, continue the reaction for 2-3 hours to obtain a modifier.

3. The thin and light warm needle-punched elastic composite material according to claim 2, characterized in that: The molar ratio of diethylenetriamine to epichlorohydrin in step (1) is 1:2-2.1; the molar ratio of diethylenetriamine chloride to dodecyldimethyl tertiary amine in step (2) is 1:1-1.1; the molar ratio of the modifier quaternary ammonium salt, diethylphosphite chloride, and triethylamine in step (3) is 1:1-1.1:1.5-2.

0.

4. The thin and light warm needle-punched elastic composite material according to claim 1, characterized in that: In the preparation method of modified polyvinyl chloride, the mass ratio of polyvinyl chloride, modifier and triethylamine is 1:0.6-0.8:0.1-0.

2.

5. The thin and light warm needle-punched elastic composite material according to claim 1, characterized in that: In the preparation method of modified polyvinyl chloride, after the reaction is completed, the temperature is naturally lowered to room temperature, glycerol is added until no precipitate is precipitated, the precipitate is filtered, and the precipitate is washed with water three times and dried to obtain the modified polyvinyl chloride.

6. The thin and light warm needle-punched elastic composite material according to claim 1, characterized in that: The mass ratio of methyltrimethoxysilane, 3-aminopropyltrimethoxysilane and the mixed solvent in step S1 is 1:0.8-1:4-5; the mixed solvent is ethanol and water in a mass ratio of 1:0.1-0.

2.

7. The light, thin, warm-keeping, needle-punched elastic composite material according to claim 1, characterized in that: The amount of the modified quaternary ammonium salt in step S2 is the same as the molar amount of 3-aminopropyltrimethoxysilane in step S1; the molar ratio of the modified quaternary ammonium salt to N,N'-carbonyldiimidazole is 1:1-1.

1.

8. A method for preparing a thin and light warm needle-punched elastic composite material according to any one of claims 1 to 7, characterized in that: By weight, the method comprises the following steps: A1. After uniformly mixing 40-50 parts of polyamide, 30-40 parts of modified polyvinyl chloride, 10-15 parts of plasticizer and 5-8 parts of heat stabilizer, add them into an internal mixer, heat them to 120-130°C, mix them for 5-10 minutes, add 60-70 parts of nitrile rubber, 2-3 parts of antioxidant and 5-10 parts of filler, continue to heat them to 150-160°C, mix them for 15-20 minutes to obtain a masterbatch; A2, adding 10-15 parts of foaming agent, 6-10 parts of vulcanizing agent, 3-5 parts of vulcanization accelerator and 30-35 parts of modified silica aerogel to the masterbatch, cooling to 90-100°C, mixing for 3-5 minutes to obtain a rubber mix; putting the rubber mix into an extruder, extruding it into a desired shape, and then putting it into a molding machine for curing, and rapidly cooling it at a speed greater than 4°C / s to obtain an elastic foam material; A3. Place needle-punched cotton fibers on one side surface of the elastic foam material or on both side surfaces of the elastic foam material or in the middle of two layers of elastic foam material, and compound them by needle-punching to obtain a composite material.

9. The method for preparing a thin and light warm needle-punched elastic composite material according to claim 8, characterized in that: The curing process in step A2 is as follows: the first curing pressure is 10-15MPa, the temperature is 130-150°C, and the time is 15-20min; the second curing pressure is 15-20MPa, the temperature is 170-180°C, and the time is 10-15min.

10. The use of a light, thin, warm, needle-punched elastic composite material according to any one of claims 1 to 7, characterized in that: The composite material is used in clothing, shoes and hats, cold chain packaging, construction, and aerospace fields.