Bare-fired permeable brick without backing plate and preparation method thereof
By using stone brick crushing materials, bentonite and other materials to make green permeable bricks, and using backing-free bare firing technology to sinter at low temperatures, the problems of high energy consumption and long cycle caused by the use of backing plates during the firing of permeable bricks are solved. , achieving an efficient and energy-saving production process.
Patent Information
- Application Number
- CN202410595137.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-14
AI Technical Summary
Existing permeable bricks require the use of backing plates during the firing process, resulting in a long firing cycle, high energy consumption and high cost, and it is difficult to achieve bare firing without backing plates.
The permeable brick green body is made of 35 to 70% of broken stone bricks and 30 to 65% of bentonite, washed sand, calcium powder and other materials, and is sintered at a temperature of 1120 to 1160°C through bare firing without a backing plate. Form a low-temperature fusion body to reduce energy consumption.
It effectively shortens the firing cycle and reduces unit energy consumption and production costs. The average energy consumption is 3.0 to 5.5 m3 of natural gas per square meter, achieving solid waste utilization and energy conservation and emission reduction.
Smart Images

Figure SMS_1 
Figure SMS_10 
Figure SMS_11
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of permeable bricks, and in particular relates to a bare-fired permeable brick without a backing plate and a preparation method thereof. Background Art
[0002] Permeable bricks (also known as seepage bricks) are a new type of building material. They can use solid waste such as waste tiles, stone fragments, slag, etc. as the main raw materials, add an appropriate amount of binder, and sinter under high temperature conditions. At present, permeable bricks are mainly ridge materials, with poor plasticity and low green strength. This requires that pads must be used to support the green body during the firing process to prevent the green body from scattering during movement in the tunnel kiln or roller kiln. However, this method will result in a long firing cycle for permeable bricks, which takes 3 to 6 hours, and high energy consumption, about 6.0 to 7.5 m per square meter of permeable bricks. 3 Natural gas. If the permeable brick can omit the backing plate during the firing process, it will be helpful to reduce the cost. Therefore, it is necessary to propose a permeable brick that is fired bare without a backing plate. Summary of the invention
[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a bare-fired permeable brick without a backing plate and a preparation method thereof, which adopts a bare-fired method without a backing plate for sintering, effectively reducing the unit energy consumption of the product, shortening the firing cycle, and reducing production costs.
[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:
[0005] In the first aspect of the present invention, the present invention provides a bare-fired permeable brick without a backing plate, which is made of a permeable brick green body. Calculated by mass percentage, the permeable brick green body includes 35-70% of a first raw material and 30-65% of a second raw material. The first raw material is a crushed material formed by stoneware bricks, and the second raw material includes bentonite, washed sand and calcium powder.
[0006] Preferably, the first raw material is crushed paving stone with a water absorption rate of 0.5-3.0%.
[0007] More preferably, the first raw material includes coarse aggregate with a particle size of 10 to 20 meshes and fine aggregate with a fineness of ≤60 meshes.
[0008] More preferably, in the first raw material, the mass ratio of coarse aggregate to fine aggregate is (2-6):1.
[0009] Preferably, the washed sand is the tailings remaining after natural feldspar is selected and washed, and has a fineness of ≤20 mesh; in the permeable brick green body, the mass percentage of the washed sand is 10-35%.
[0010] Preferably, in the permeable brick green body, the mass percentage of bentonite is 10-20%, the content of aluminum oxide in the bentonite is ≥10%, and the dry strength of the bentonite is ≥5.0 MPa.
[0011] Preferably, in the permeable brick green body, the mass percentage of calcium powder is 5-10%, and the calcium powder includes one or more of lime powder, double fly ash powder, calcite powder and marble powder.
[0012] Preferably, the second raw material also includes talcum powder, and the mass percentage of talcum powder in the permeable brick green body is 5-10%.
[0013] More preferably, the talc powder comprises white talc with a particle size of ≤10 mesh.
[0014] In a second aspect of the present invention, the present invention provides a method for preparing a bare-fired water-permeable brick without a backing plate, the steps being as follows:
[0015] The first raw material is crushed, and then water is added and mixed evenly to obtain a first raw material mixture;
[0016] Mixing the second raw material uniformly to obtain a second raw material mixture;
[0017] The first raw material mixture and the second raw material mixture are evenly mixed and pressed into shape to obtain a permeable brick green body;
[0018] The permeable brick green body is fired in a roller kiln without a backing plate at a temperature of 1120-1160°C to obtain the permeable brick.
[0019] Beneficial effects:
[0020] The present invention adopts a naked firing method for sintering, without a pad, and the sintering temperature of the first raw material of the paving stone supplemented with the second raw material will have a lower sintering temperature of only 1120-1160°C. The washed sand, calcium powder and talc in the second raw material are easy to form a low-temperature eutectic body, so it is generally 30-50°C lower than the pad firing temperature, which can effectively reduce the unit energy consumption of the product and reduce the production cost. The firing cycle is 2-3.5 hours, and the average energy consumption is about 3.0-5.5 m2 per square meter of permeable brick. 3 Natural gas is beneficial to solid waste utilization and energy conservation and emission reduction. DETAILED DESCRIPTION
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the specific implementation methods of the present invention will be described below. Obviously, the following descriptions are only some embodiments of the present invention, and for those of ordinary skill in the art, other implementation methods can also be obtained based on these embodiments without creative work.
[0022] The invention provides a bare-fired permeable brick without a backing plate, which is made of a permeable brick green body. Calculated by mass percentage, the permeable brick green body includes 35-70% of a first raw material and 30-65% of a second raw material. The first raw material is a crushed material formed by a stoneware brick, and the second raw material includes bentonite, washed sand and calcium powder.
[0023] The first raw material is clinker. The permeable bricks produced by the present invention have high strength after drying, and their flexural strength is ≥0.5MPa, which can meet the requirements of roller kiln bare firing. The second raw material of the present invention uses raw material to replace the conventional "binder + flux". During the firing process, new substances will be formed to wrap the first raw material at high temperature, effectively enhancing the strength of the green body. Stoneware bricks have good water permeability. The present invention uses a first raw material with high water permeability, so that the first raw material is more closely combined with the second raw material at high temperature.
[0024] Preferably, the first raw material is crushed paving stone with a water absorption rate of 0.5-3.0%. The paving stone used in the present invention is a porous lightweight brick, which is a sintered paving stone with a honeycomb structure. It is breathable, water-permeable and lightweight and can be used as an aggregate. The first raw material with high water permeability has a larger contact surface with the second raw material when preparing the green body, which is beneficial to improve the strength of the green body, and the molten material formed by the reaction of the second raw material at high temperature can be better combined with the first raw material with high water permeability.
[0025] The crushed floor stone material can be made by crushing waste floor stone bricks containing glaze, so as to realize the utilization of solid waste. Generally speaking, the glaze on the surface of floor stone is to imitate porcelain bricks. The glaze is a thin layer of glass, containing silicate minerals, flux, stabilizer, pigment and colorant, etc. The first raw material with glaze is melted together with the second raw material during sintering. It should be noted that the present invention does not limit the specific composition of the first raw material. The first raw material is clinker and does not participate in the reaction during the sintering process. Therefore, the present invention only limits the water absorption rate of the first raw material. When the first raw material is floor stone, the glaze content on the surface of the floor stone is very small. The composition of common glazes is close, but there is a difference in content. The present invention does not prepare the green body of permeable bricks through glaze. The glaze is only attached to the surface of the floor stone. Therefore, the present invention does not limit the glaze.
[0026] In the present invention, the role of the first raw material is mainly to improve the strength of the green body and to improve the product performance by mixing with the molten second raw material. In some embodiments, the first raw material is a graded ingredient, including coarse aggregate of 10 to 20 mesh and fine aggregate of less than or equal to 60 mesh. The present invention uses particles of 10 to 20 mesh instead of coarser particles of 4 to 10 mesh, which effectively avoids the friction between the first raw material and the roller rod when the first raw material and the second raw material are mixed, resulting in slag falling and scattering. The present invention incorporates fine aggregate of ≤60 mesh, the fine aggregate is melted into the molten second raw material, and the molten second raw material then wraps the coarse aggregate, so that the overall flexural strength of the product is improved. In addition, when preparing the green body, in the process of mixing the first raw material and the second raw material, the fine aggregate is mixed into the second raw material, and the second raw material then wraps the coarse aggregate, so that the composition of the green body is uniform and the firing quality is good.
[0027] Preferably, in the first raw material, the mass ratio of coarse aggregate to fine aggregate is (2-6):1.
[0028] In the present invention, the strength of the green brick of the permeable brick is relatively high, and it can be fired without a backing plate. Compared with the existing method of firing the green brick with a backing plate, the present invention can avoid the loss of heat during the backing plate transfer process. In addition, the second raw material of the present invention forms a low-temperature eutectic during the firing process, which is 30 to 50°C lower than the conventional backing firing temperature, effectively reducing the unit energy consumption of the product. The firing cycle of the present invention is 2 to 3.5 hours, and the average energy consumption is about 3.0 to 5.5 m2 per square meter of permeable brick. 3 Natural gas has greatly reduced production costs.
[0029] In the present invention, washed sand is the tailings remaining after natural feldspar is carefully washed, and the particle size is ≤20 mesh. The washed sand contains sodium and potassium, which is conducive to the formation of a low-temperature eutectic body with the second raw material. Preferably, in the green body of permeable bricks, the mass percentage of washed sand is 10-35%. Washed sand is feldspar, which can also be used as aggregate. Specifically, the tailings remaining after natural feldspar is carefully washed have different particle sizes. Among them, the coarse particles play the role of aggregates, which are beneficial to improve the strength of the product after sintering, and the fine particles play the role of auxiliary materials.
[0030] Bentonite acts as a binder, which is beneficial to enhancing the strength of the permeable brick green body. Preferably, the dry strength of bentonite is ≥5.0 MPa, and more preferably, the dry strength of bentonite is ≥10 MPa. Bentonite has a high silicon content, which can reduce the sintering temperature and is beneficial to the second raw material to form a low-temperature eutectic. Preferably, the content of aluminum oxide in bentonite is ≥10% to avoid the sintering temperature being too low, which affects the permeability of the product. Preferably, in the permeable brick green body, the mass percentage of bentonite is 10-20%, and more preferably, the mass percentage of bentonite is 10-15%.
[0031] Calcium powder plays the role of porogen. In the present invention, calcium powder includes one or more of lime powder, double fly ash powder, calcite powder and marble powder, and the main component is calcium carbonate. Preferably, the present invention uses cutting powder produced by marble processing to realize solid waste utilization. Preferably, in the permeable brick green body, the mass percentage of calcium powder is 5-10%.
[0032] In the present invention, the second raw material also includes talc powder, which also acts as a low-temperature flux, and conventional commercially available talc is used, preferably white talc with a particle size of ≤10 mesh. Preferably, in the permeable brick green body, the mass percentage of talc powder is 5-10%.
[0033] In the present invention, calcium powder and washed sand are waste materials generated in the production process of other related products, and are combined with crushed paving stones to form green permeable bricks, which is beneficial to solid waste recycling, reducing production costs, and also beneficial to environmental protection.
[0034] The present invention also provides a method for preparing a bare-fired water-permeable brick without a backing plate, which is as follows:
[0035] The first raw material is crushed, sieved to obtain coarse aggregate and fine aggregate, the coarse aggregate and the fine aggregate are mixed evenly, and then water is added to mix evenly again to obtain a first raw material mixture;
[0036] Mixing the second raw material uniformly to obtain a second raw material mixture;
[0037] The first raw material mixture and the second raw material mixture are evenly mixed and pressed into shape to obtain a permeable brick green body;
[0038] The permeable brick green body is fired in a roller kiln without a backing plate at a temperature of 1120-1160°C to produce the permeable brick.
[0039] Wherein, when preparing the first raw material mixture, the mass ratio of the amount of water added to the permeable brick green body is 0.03-0.07, that is, in the pressing step, the present invention adopts a dry pressing process.
[0040] The technical solution of the present invention is described in detail below with specific embodiments.
[0041] The first raw material is crushed paving stone with a water absorption rate of 2%;
[0042] Washed sand is the tailings left over from washing natural feldspar, with a particle size of ≤20 mesh;
[0043] The bentonite is commercially available calcium-based bentonite. The composition and content of the calcium-based bentonite are: 12.65% aluminum oxide, 69.22% silicon dioxide, 1.18% iron oxide, 3.67% calcium oxide, 3.71% magnesium oxide, 0.73% potassium oxide, 0.37% sodium oxide and 0.19% titanium dioxide. The loss on ignition is 8.14%, and the rest are trace elements.
[0044] Calcium powder is the cutting powder produced by marble processing, with a particle size of ≤10 mesh;
[0045] The talc is commercially available white talc, and the composition and content of the white talc are 2.67% aluminum oxide, 60.84% silicon dioxide, 0.28% iron oxide, 0.94% calcium oxide, 33.83% magnesium oxide, 0.69% potassium oxide, 0.07% sodium oxide and 0.08% titanium dioxide, the loss on ignition is 0.31%, and the rest are trace elements.
[0046] Example 1
[0047] The first raw material includes coarse aggregate of 10-20 mesh and fine aggregate below 60 mesh, and the second raw material includes washed sand, bentonite, white talc and calcium powder. The first raw material and the second raw material are mixed according to the formula in Table 1, taking the total weight of 1 kg as an example.
[0048] Table 1 The ratio of the first raw material and the second raw material in Example 1
[0049]
[0050] Weigh the coarse aggregate and fine aggregate according to the formula in Table 1, mix them evenly, add 7% of water to the total amount, mix evenly, and obtain a first raw material mixture;
[0051] Weigh the second raw material according to the formula in Table 1, mix them evenly, and obtain a second raw material mixture;
[0052] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a permeable brick green body, which is then placed in an oven for drying.
[0053] The dried green body was taken and its flexural strength was tested. The results are shown in Table 2.
[0054] Table 2 Flexural strength of the green permeable brick of Example 1
[0055]
[0056] Note: The flexural strength test standard is "T / CBCSA 13-2019 Sintered Permeable Brick Standard".
[0057] According to the data in Table 2, the green bodies of the three formulations in Example 1 all meet the strength requirements for sintering without a backing plate (it is believed in the art that green bodies with a flexural strength greater than or equal to 0.5 MPa can be fired bare).
[0058] The green body was fired in a kiln at a sintering temperature of 1130°C to obtain a finished product. The test results are as follows. The flexural strength, compressive strength and water permeability coefficient of the finished product are shown in Table 3, all of which meet the requirements of "T / CBCSA 13-2019 Sintered Permeable Brick Standard".
[0059] Specifically, the "T / CBCSA 13-2019 Sintered Permeable Brick Standard" requires: flexural strength ≥ 6MPa, compressive strength ≥ 35 MPa, permeability coefficient ≥ 1.0×10 -2 cm / s.
[0060] Table 3 Performance of the permeable bricks of Example 1
[0061]
[0062] Example 2
[0063] The first raw material includes coarse aggregate of 10-20 mesh and fine aggregate below 60 mesh, and the second raw material includes washed sand, bentonite and calcium powder. The first raw material and the second raw material are mixed according to the formula in Table 4, taking the total weight of 1 kg as an example.
[0064] Table 4 The proportions by mass of the first raw material and the second raw material in Example 2.
[0065]
[0066] Weigh the coarse aggregate and fine aggregate according to the formula in Table 4, mix them evenly, add 7% of water, mix them evenly, and obtain a first raw material mixture;
[0067] Weigh the second raw material according to the formula in Table 4, mix them evenly, and obtain a second raw material mixture;
[0068] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a green body, which is placed in an oven for drying.
[0069] The dried green body was taken and its flexural strength was tested. The results are shown in Table 5.
[0070] Table 5 Flexural strength of the green permeable brick of Example 2
[0071]
[0072] According to the data in Table 5, the green bodies of the four formulations in Example 2 all meet the strength requirements of sintering without a backing plate.
[0073] The green body was fired in a kiln at a sintering temperature of 1140°C to obtain a finished product. The test results are as follows. The flexural strength, compressive strength and water permeability coefficient of the finished product are shown in Table 6, all of which meet the requirements of "T / CBCSA 13-2019 Sintered Permeable Brick Standard".
[0074] Table 6 Performance of the permeable bricks of Example 2
[0075]
[0076] Comparative Example 1
[0077] The first raw material includes coarse aggregate of 10 to 20 meshes and fine aggregate below 60 meshes, and the second raw material includes washed sand, other fluxes and other binders. Among them, the composition and content of the flux used in this comparative example are: 15.54% aluminum oxide, 65.74% silicon dioxide, 2.78% iron oxide, 1.66% calcium oxide, 2.66% magnesium oxide, 1.82% potassium oxide, 1.32% sodium oxide and 0.26% titanium dioxide, the loss on ignition is 8.03%, and the rest are trace elements; the composition and content of the binder used in this comparative example are: 2.11% aluminum oxide, 72.07% silicon dioxide, 0.10% iron oxide, 5.26% calcium oxide, 2.99% magnesium oxide, 1.33% potassium oxide, 13.01% sodium oxide and 0.06% titanium dioxide, the loss on ignition is 0.70%, and the rest are trace elements. The first raw material and the second raw material are mixed according to the formula in Table 7, taking the total weight of the ingredients as 1 kg as an example.
[0078] Table 7 Ratio of the first raw material and the second raw material in comparative example 1
[0079]
[0080] Weigh the coarse aggregate and the fine aggregate according to the formula in Table 7, mix them evenly, add 7% of water to the total amount, mix them evenly, and obtain a first raw material mixture;
[0081] Weigh the second raw material according to the formula in Table 7, mix them evenly, and obtain a second raw material mixture;
[0082] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a green body, which is placed in an oven for drying.
[0083] The dried green body was taken and its flexural strength was tested. The results are shown in Table 8.
[0084] Table 8 Flexural strength of green body of Comparative Example 1
[0085]
[0086] According to the data in Table 8, the green bodies of the three formulations in Comparative Example 1 all meet the strength requirements of sintering without a backing plate.
[0087] In this comparative example, the aluminum content of the binder is much lower than the aluminum content of the bentonite in the example. The low aluminum content leads to a decrease in the sintering temperature. In addition, the high sodium content in the binder also significantly reduces the sintering temperature of this comparative example.
[0088] While ensuring other performance of the product, the green body is fired in a kiln at a sintering temperature of 1130°C to obtain a finished product. However, at this temperature, it is sintered densely and is tested to be impermeable to water.
[0089] Comparative Example 2
[0090] The porcelain polished tile aggregate is crushed and sieved to obtain aggregate particles with a particle size of 10-20 mesh and below 60 mesh, which are coarse porcelain aggregate and fine porcelain aggregate respectively.
[0091] The auxiliary materials include washed sand, bentonite and calcium powder. The aggregate and auxiliary materials of porcelain polished tiles are mixed according to the formula in Table 9, taking the total weight of 1 kg as an example.
[0092] Table 9 Proportion by mass of aggregate and auxiliary materials for polished porcelain tiles in Comparative Example 2
[0093]
[0094] Weigh the coarse porcelain aggregate and the fine porcelain aggregate according to the formula in Table 9, mix them evenly, add 7% of water to the total amount, mix them evenly, and obtain an aggregate mixture;
[0095] Weigh the auxiliary materials according to the formula in Table 9, mix them evenly, and obtain an auxiliary material mixture;
[0096] Add the auxiliary material mixture to the aggregate mixture and mix them evenly so that the auxiliary material mixture is evenly wrapped on the surface of the aggregate particles. Use a permeable brick press to press and form the green body. The press pressure is set to 1500 T to obtain the green body, which is then placed in an oven for drying.
[0097] The dried green body was taken and its flexural strength was tested. The results are shown in Table 10.
[0098] Table 10 Flexural strength of green body of comparative example 2
[0099]
[0100] According to the data in Table 10, the green bodies of the two formulations in Comparative Example 2 both meet the strength requirements for sintering without a backing plate.
[0101] The green body was fired in a kiln at a sintering temperature of 1140°C to obtain a finished product. The test results are shown in Table 11. The finished product has slight water seepage and the water permeability coefficient cannot meet the requirements of "T / CBCSA 13-2019 Sintered Permeable Brick Standard".
[0102] Table 11 Performance of the bricks produced in Comparative Example 2
[0103]
[0104] Comparative Example 3
[0105] In this comparative example, the first raw material includes coarse aggregate of 10-20 mesh and fine aggregate of less than 60 mesh, and the second raw material includes washed sand, bentonite, white talc and calcium powder. The total weight of the first raw material and the second raw material is 1 kg.
[0106] Among them, calculated by mass percentage, coarse aggregate is 20%, fine aggregate is 10%, washed sand is 20%, bentonite is 20%, white talc is 20%, and calcium powder is 10%.
[0107] Weigh the coarse aggregate and the fine aggregate, mix them evenly, add 7% of water, mix them evenly, and obtain a first raw material mixture;
[0108] Weigh the second raw material, mix it evenly, and obtain a second raw material mixture;
[0109] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a permeable brick green body, which is then placed in an oven for drying.
[0110] The dried green body was taken out and its flexural strength was tested. The flexural strength of the green body was 0.7242 MPa.
[0111] The green body is fired in a kiln at a sintering temperature of 1130°C to obtain a finished product. The finished product has no cracks on the surface, the surface is molten, and it is not permeable, which does not meet the permeable performance requirements of permeable bricks.
[0112] Comparative Example 4
[0113] In this comparative example, the first raw material includes coarse aggregate of 10-20 mesh and fine aggregate of less than 60 mesh, and the second raw material includes washed sand, bentonite, white talc and calcium powder. The total weight of the first raw material and the second raw material is 1 kg.
[0114] Among them, calculated by mass percentage, coarse aggregate is 50%, fine aggregate is 30%, washed sand is 5%, bentonite is 5%, white talc is 5%, and calcium powder is 5%.
[0115] Weigh the coarse aggregate and the fine aggregate, mix them evenly, add 7% of water, mix them evenly, and obtain a first raw material mixture;
[0116] Weigh the second raw material, mix it evenly, and obtain a second raw material mixture;
[0117] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a permeable brick green body, which is then placed in an oven for drying.
[0118] The dried green body was taken and its flexural strength was tested. The flexural strength of the green body was 0.6034 MPa.
[0119] The green body is fired in a kiln at a sintering temperature of 1130°C to obtain a finished product. The surface of the finished product has many cracks, which does not meet the requirement of non-penetrating cracks ≦2 for the appearance quality of permeable bricks.
[0120] Comparative Example 5
[0121] In this comparative example, the first raw material is 10-20 mesh coarse aggregate, and the second raw material includes washed sand, bentonite, white talc and calcium powder. The total weight of the first raw material and the second raw material is 1 kg.
[0122] Among them, calculated by mass percentage, the first raw material is 60%, washed sand is 15%, bentonite is 10%, white talc is 10%, and calcium powder is 5%.
[0123] Weigh the first raw material, add 7% of water to the total amount, mix well, and obtain a first raw material mixture;
[0124] Weigh the second raw material, mix it evenly, and obtain a second raw material mixture;
[0125] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a permeable brick green body, which is then placed in an oven for drying.
[0126] The dried green body was taken out and its flexural strength was tested. The flexural strength of the green body was 0.5549 MPa.
[0127] The green body is fired in a kiln at a sintering temperature of 1130°C to obtain a finished product. The finished product has cracks on its surface, which does not meet the requirement of non-penetrating cracks ≦2 in the appearance quality of permeable bricks.
[0128] Comparative Example 6
[0129] In this comparative example, the first raw material is fine aggregate with a mesh size of less than 60, and the second raw material includes washed sand, bentonite, white talc and calcium powder. The total weight of the first raw material and the second raw material is 1 kg.
[0130] Among them, calculated by mass percentage, the first raw material is 60%, washed sand is 15%, bentonite is 10%, white talc is 10%, and calcium powder is 5%.
[0131] Weigh the first raw material, add 7% of water to the total amount, mix well, and obtain a first raw material mixture;
[0132] Weigh the second raw material, mix it evenly, and obtain a second raw material mixture;
[0133] The second raw material mixture is added to the first raw material mixture, mixed evenly, so that the second raw material mixture is evenly wrapped on the surface of the first raw material particles, and pressed into shape using a permeable brick press, with the press pressure set to 1500 F, to obtain a permeable brick green body, which is then placed in an oven for drying.
[0134] The dried green body was taken and its flexural strength was tested. The flexural strength of the green body was 0.8937 MPa.
[0135] The green body was fired in a kiln at a sintering temperature of 1130°C to obtain a finished product. The test results are as follows: the flexural strength of the finished product is 8.4 MPa, the compressive strength is 66.4 MPa and the water permeability coefficient is 0.6×10 -2 cm / s, the water permeability coefficient does not reach the water permeability coefficient of permeable bricks 1.0×10 -2 cm / s requirement.
[0136] The embodiments provided by the present invention are described in detail above. Specific examples are used herein to describe the principles and implementation methods of the present invention, and the description of the above embodiments is only used to help understand the core idea of the present invention. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A bare-fired permeable brick without a backing plate, characterized in that: The permeable brick green body is made by firing the green body without a backing plate in a roller kiln. Calculated by mass percentage, the green body of the permeable brick includes 35-70% of the first raw material and 30-65% of the second raw material. The first raw material is composed of coarse aggregate with a particle size of 10-20 meshes and fine aggregate with a particle size of ≤60 meshes. The second raw material includes bentonite, washed sand and calcium powder. The first raw material is crushed paving stone formed by stoneware bricks with a water absorption rate of 0.5-3.0%, and the mass ratio of coarse aggregate to fine aggregate in the first raw material is (2-6):1; The washed sand is the tailings remaining after natural feldspar is carefully washed, with a fineness of ≤20 mesh; Wherein, the calcium powder includes one or more of lime powder, double fly powder, calcite powder and marble powder; Wherein, in the second raw material, the content of aluminum oxide in the bentonite is ≥10%; In the permeable brick green body, the mass percentage of the washed sand is 10-35%, the mass percentage of the bentonite is 10-20%, and the mass percentage of the calcium powder is 5-10%; The method for preparing the green body of the permeable brick is as follows: crushing the first raw material, mixing it evenly, then adding water and mixing it evenly again to obtain a first raw material mixture; Mixing the second raw material uniformly to obtain a second raw material mixture; The first raw material mixture and the second raw material mixture are evenly mixed and pressed into shape to obtain a permeable brick green body.
2. The bare-fired permeable brick without backing plate according to claim 1 is characterized in that: The dry strength of the bentonite is ≥5.0 MPa.
3. The bare-fired permeable brick without backing plate according to claim 1 is characterized in that: The second raw material also includes talcum powder. In the green body of the permeable brick, the mass percentage of the talcum powder is 5-10%.
4. The bare-fired permeable brick without backing plate according to claim 3 is characterized in that: The talc powder includes white talc with a particle size of ≤10 mesh.
5. A method for preparing bare-fired permeable bricks without backing plates, characterized in that: The steps for preparing the bare-fired permeable brick without backing plate as claimed in any one of claims 1 to 4 are as follows: The first raw material is crushed and mixed evenly, and then water is added and mixed evenly again to obtain a first raw material mixture; Mixing the second raw material uniformly to obtain a second raw material mixture; The first raw material mixture and the second raw material mixture are evenly mixed and pressed into shape to obtain a permeable brick green body; The permeable brick green body is fired in a roller kiln without a backing plate at a temperature of 1120-1160°C to obtain the permeable brick.
Citation Information
Patent Citations
Ceramic tile with porous structure at bottom and preparation method of ceramic tile
CN110054475A
Water-permeable block for pavement and its production
JP1998152382A