Preparation method of polyurethane emulsion
After removal of water by polypropylene glycol and polybutylene adipate diol, react with isocyanate and organic bismuth catalyst, combining hydrophilic chain extender and neutralizer, and finally with isofolonediamine and N-2- Aminoethyl-3-aminopropyltriethoxysilane reaction forms a polyurethane emulsion with high solid content and low viscosity, solving the problems of environmental pollution and insufficient performance in the prior art, and achieving high mechanical properties and solvent resistance .
Patent Information
- Application Number
- CN202410358899.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-03-27
AI Technical Summary
There are problems of environmental pollution and insufficient performance in the existing polyurethane emulsion preparation methods, including high viscosity, low mechanical strength and adhesive strength, and easy to dissolve in solvents.
After removing water, polypropylene glycol and polybutylene adipate diol glycol react with isocyanate and organic bismuth catalyst to form a prepolymer, followed by addition of hydrophilic chain extender and neutralizer, further emulsification treatment, and finally with isoplasmic Fluoronediamine reacts with N-2-aminoethyl-3-aminopropyltriethoxysilane to form a polyurethane emulsion with high solids content and low viscosity.
The high solid content, low viscosity and good mechanical properties of the polyurethane emulsion are achieved, which reduces the cost of drying and curing and transportation, improves the convenience of construction operations, and enhances the solvent resistance after film formation.
Smart Images

Figure BDA0004762226350000021 
Figure BDA0004762226350000031 
Figure BDA0004762226350000041
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a polyurethane emulsion. Background Art
[0002] Polyurethane has excellent toughness, wear resistance, low temperature resistance and impact resistance, and its application field is wide and the demand is large. At present, most commercially available polyurethanes contain a certain amount of organic solvents. For example, CN102408536A discloses a method for preparing a polyurethane-urea dispersion, in which polyols, polyethylene glycol, hydrophilic chain extenders, polyisocyanates and catalysts are reacted to generate polyurethane-urea prepolymers, the polyurethane prepolymers are diluted with organic solvents, the chains are extended with a mixture of polyamines, distilled water or deionized water is added under mechanical stirring for emulsification and dispersion, and the solvent is removed under reduced pressure. These products will release a certain amount of volatile organic matter during the preparation and use process, causing environmental pollution and affecting human health.
[0003] CN102702471A discloses a method for preparing a solvent-free waterborne polyurethane dispersion, comprising mixing polyisocyanate, carboxyl-containing small molecule diol, small molecule diol, polyol and an organic metal catalyst, stirring and reacting to obtain a prepolymer containing terminal isocyanate groups; adding water to the prepolymer and stirring for 3 to 10 minutes; mixing tertiary amine and water, adding the mixture to the reaction system, and continuing to stir; then adding an amine chain extender and water to the reaction system, stirring and reacting to obtain a waterborne polyurethane dispersion. The polyurethane dispersion obtained by the method has low mechanical strength and bonding strength after film formation.
[0004] CN107417873B discloses a method for preparing an aqueous polyurethane dispersion, comprising reacting at least one polyhydroxy oligomer polyol, at least one polyisocyanate and a small molecule hydrophilic chain extender to obtain a polyurethane prepolymer with an NCO group at the end; then reacting the polyurethane prepolymer with an NCO group at the end with a small molecule neutralizer, adding deionized water at 60-100°C, lowering the temperature of the reaction system to 20-50°C after dispersion under stirring, and then adding deionized water to obtain a prepolymer dispersion after dispersion; finally, reacting the prepolymer dispersion with a sulfonate type polyamine hydrophilic chain extender, and then reacting with a polyamine chain extender to obtain an aqueous polyurethane dispersion. The aqueous polyurethane dispersion has a high viscosity, is not easy to construct and operate, and has a low bonding strength. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a method for preparing a polyurethane emulsion, which can obtain a polyurethane emulsion with high solid content and low viscosity. Furthermore, the polyurethane emulsion obtained by the preparation method has high mechanical strength and bonding strength after film formation. Furthermore, the polyurethane emulsion obtained by the preparation method has good solvent resistance after film formation.
[0006] The present invention achieves the above-mentioned purpose through the following technical solutions.
[0007] The present invention provides a method for preparing a polyurethane emulsion, comprising the following steps:
[0008] (1) removing water from 15 to 35 parts by weight of polypropylene glycol and 30 to 50 parts by weight of polybutylene adipate diol to obtain dehydrated polypropylene glycol and dehydrated polybutylene adipate diol;
[0009] (2) reacting the dehydrated polypropylene glycol, the dehydrated polybutylene adipate glycol, 5 to 15 parts by weight of a first diisocyanate, 12 to 25 parts by weight of a second diisocyanate, and 0.03 to 0.2 parts by weight of an organic bismuth catalyst to obtain a primary prepolymer;
[0010] Wherein, the first diisocyanate is as shown in formula (A):
[0011]
[0012] In formula (A), m is an integer selected from 1 to 8;
[0013] Wherein, the second diisocyanate is as shown in formula (B):
[0014]
[0015] In formula (B), R1 is selected from C1-C6 alkylene, and R2-R9 are independently selected from H or C1-C6 alkyl;
[0016] (3) reacting the primary prepolymer, 2 to 15 parts by weight of a hydrophilic chain extender and 0.5 to 3 parts by weight of a neutralizing agent to obtain a secondary prepolymer;
[0017] (4) emulsifying the secondary prepolymer in the presence of an emulsifier, and then adding water for further emulsification to obtain an emulsified product; the emulsifier includes water and sodium fatty alcohol polyoxyethylene ether carboxylate;
[0018] (5) The emulsified product, 2 to 8 parts by weight of isophorone diamine and 1 to 5 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane are reacted to obtain a polyurethane emulsion.
[0019] According to the preparation method of the present invention, preferably, in formula (A), m is selected from an integer of 2 to 6; in formula (B), R1 is selected from an alkylene group of C1 to C3, and R2 to R9 are independently selected from H or an alkyl group of C1 to C3; the organic bismuth catalyst is selected from one or more of bismuth neodecanoate, bismuth isooctanoate, and bismuth laurate.
[0020] According to the preparation method of the present invention, preferably, the first diisocyanate is hexamethylene diisocyanate, and the second diisocyanate is 4,4'-diisocyanate dicyclohexylmethane.
[0021] According to the preparation method of the present invention, preferably, in step (2), the polypropylene glycol after dehydration at a temperature ≤ 70°C, the polybutylene adipate diol after dehydration at a temperature ≤ 70°C, the first diisocyanate, the second diisocyanate and the organic bismuth catalyst are mixed, and then reacted at 70 to 95°C for 1 to 10 hours under stirring.
[0022] According to the preparation method of the present invention, preferably, in step (3), the primary prepolymer at a temperature of ≤45° C., the hydrophilic chain extender and the neutralizing agent are mixed, and then reacted at 50 to 75° C. for 0.5 to 4 hours.
[0023] According to the preparation method of the present invention, preferably, the hydrophilic chain extender is as shown in formula (C):
[0024]
[0025] In formula (C), R 10 and R 11 are independently selected from C1 to C6 alkylene groups, and Q is selected from an integer of 1 to 6;
[0026] The neutralizing agent is selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin.
[0027] According to the preparation method of the present invention, preferably, in the emulsifier, water is 15 to 45 parts by weight, and sodium fatty alcohol polyoxyethylene ether carboxylate is 0.5 to 3 parts by weight.
[0028] According to the preparation method of the present invention, preferably, in step (4), the secondary prepolymer is emulsified in the presence of an emulsifier for 1 to 10 minutes, and then 40 to 75 parts by weight of water are added for further emulsification for 5 to 20 minutes.
[0029] According to the preparation method of the present invention, preferably, in step (5), the reaction temperature is 15 to 38° C., and the reaction time is 0.5 to 3 h.
[0030] According to the preparation method of the present invention, preferably, the solid content of the polyurethane emulsion is ≥45wt% and the viscosity is ≤700cP.
[0031] The method of the present invention is used to prepare the polyurethane emulsion, and no organic solvent is needed in the preparation process, thereby reducing the release of volatile organic matter in the preparation and use process. The preparation method of the present invention can obtain a polyurethane emulsion with high solid content and low viscosity, which reduces the cost of drying, curing and transportation, and reduces the difficulty of construction operation. The polyurethane emulsion obtained by the preparation method of the present invention has good mechanical properties and bonding strength after film formation, and has certain solvent resistance. DETAILED DESCRIPTION
[0032] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0033] The method for preparing the polyurethane emulsion of the present invention comprises the following steps: (1) a pretreatment step; (2) a step of obtaining a primary prepolymer; (3) a step of obtaining a secondary prepolymer; (4) a step of obtaining an emulsified product; and (5) a step of obtaining the polyurethane emulsion. The following is a detailed description.
[0034] <Pre-processing steps>
[0035] 15 to 35 parts by weight of polypropylene glycol and 30 to 50 parts by weight of polybutylene adipate diol are dehydrated to obtain dehydrated polypropylene glycol and dehydrated polybutylene adipate diol.
[0036] In the present invention, the amount of polypropylene glycol used is preferably 20 to 30 parts by weight; more preferably 25 to 28 parts by weight.
[0037] The molecular weight of the polypropylene glycol may be 500 to 3000, preferably 1000 to 2500, and more preferably 1500 to 2000.
[0038] In the present invention, the amount of polybutylene adipate diol used is preferably 35 to 45 parts by weight; more preferably 40 to 42 parts by weight.
[0039] The molecular weight of polybutylene adipate diol may be 500 to 4000, preferably 1000 to 3500, and more preferably 2000 to 3000.
[0040] The polypropylene glycol and polybutylene adipate glycol may be dehydrated at 100 to 150°C; preferably 120 to 130°C.
[0041] The water removal time may be 1 to 5 hours, preferably 1.5 to 3 hours.
[0042] The water removal can be carried out under vacuum conditions. Vacuum means that the pressure is ≤10Pa; preferably, the pressure is ≤1Pa; more preferably, the pressure is ≤10 -1 Pa.
[0043] The polypropylene glycol and polybutylene adipate glycol after dehydration can be cooled to a suitable temperature under the protection of an inert gas. Examples of the inert gas include, but are not limited to, nitrogen.
[0044] <Step of Obtaining a Primary Prepolymer>
[0045] The dehydrated polypropylene glycol, the dehydrated polybutylene adipate glycol, 5 to 15 parts by weight of the first diisocyanate, 12 to 25 parts by weight of the second diisocyanate and 0.03 to 0.2 parts by weight of the organic bismuth catalyst are reacted to obtain a primary prepolymer.
[0046] The first diisocyanate of the present invention is shown in formula (A):
[0047]
[0048] In formula (A), m is selected from integers of 1 to 8; preferably, m is selected from integers of 2 to 6; more preferably, m is selected from integers of 3 to 4.
[0049] According to one embodiment of the present invention, the first diisocyanate is hexamethylene diisocyanate.
[0050] The amount of the first diisocyanate used is preferably 7 to 12 parts by weight; more preferably 8 to 10 parts by weight.
[0051] The second diisocyanate of the present invention is shown in formula (B):
[0052]
[0053] In formula (B), R1 is selected from C1-C6 alkylene, and R2-R9 are independently selected from H or C1-C6 alkyl. Preferably, R1 is selected from C1-C3 alkylene. Preferably, R2-R9 are independently selected from H or C1-C3 alkyl. More preferably, R1 is selected from C1-C2 alkylene. More preferably, R2-R9 are H.
[0054] Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 2,3-dimethylbutyl, 2,2-dimethylbutyl.
[0055] Examples of alkylene groups include, but are not limited to, methylene, ethylene, n-propylene, isopropylene, n-butylene, isobutylene, n-pentylene, isopentylene, neopentylene, n-hexylene, 2-methylpentylene, 3-methylpentylene, 2,3-dimethylbutylene, 2,2-dimethylbutylene.
[0056] According to one embodiment of the present invention, the second diisocyanate is 4,4'-diisocyanate dicyclohexylmethane.
[0057] The amount of the second diisocyanate is preferably 15 to 20 parts by weight; more preferably 17 to 18 parts by weight.
[0058] The organic bismuth catalyst can be selected from one or more of bismuth neodecanoate, bismuth isooctanoate, and bismuth laurate. According to one embodiment of the present invention, the catalyst is bismuth isooctanoate.
[0059] The amount of the organic bismuth catalyst used may be 0.03 to 0.2 parts by weight, preferably 0.05 to 0.15 parts by weight, and more preferably 0.08 to 0.1 parts by weight.
[0060] The reaction temperature may be 70 to 95° C., preferably 75 to 90° C., and more preferably 80 to 85° C. The reaction time may be 1 to 10 h, preferably 2 to 8 h, and more preferably 3 to 4 h. The reaction may be carried out under stirring.
[0061] In some embodiments, the polypropylene glycol after dehydration at a temperature of ≤70°C, the polybutylene adipate diol after dehydration at a temperature of ≤70°C, the first diisocyanate, the second diisocyanate and the organic bismuth catalyst can be mixed. Preferably, the temperature of the polypropylene glycol after dehydration is ≤60°C. In some embodiments, the temperature of the polypropylene glycol after dehydration is 20 to 60°C. Preferably, the temperature of the polybutylene adipate diol after dehydration is ≤60°C. In some embodiments, the temperature of the polybutylene adipate diol after dehydration is 20 to 60°C.
[0062] <Step of Obtaining Secondary Prepolymer>
[0063] The primary prepolymer, 2 to 15 parts by weight of a hydrophilic chain extender and 0.5 to 3 parts by weight of a neutralizing agent are reacted to obtain a secondary prepolymer.
[0064] The hydrophilic chain extender of the present invention can be shown as formula (C):
[0065]
[0066] In formula (C), R 10 and R 11 are independently selected from C1 to C6 alkylene groups, and Q is selected from an integer of 1 to 6. Preferably, R 10 and R 11 are independently selected from C1 to C3 alkylene groups. More preferably, R 10 and R 11 Preferably, Q is selected from an integer of 1-3; more preferably, Q is selected from an integer of 1-2.
[0067] Examples of alkylene groups include, but are not limited to, methylene, ethylene, n-propylene, isopropylene, n-butylene, isobutylene, n-pentylene, isopentylene, neopentylene, n-hexylene, 2-methylpentylene, 3-methylpentylene, 2,3-dimethylbutylene, 2,2-dimethylbutylene.
[0068] According to one embodiment of the present invention, the hydrophilic chain extender is dimethylolbutyric acid.
[0069] The amount of the hydrophilic chain extender is preferably 5 to 10 parts by weight; more preferably 7 to 8 parts by weight.
[0070] The neutralizing agent can be selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin. According to one embodiment of the present invention, the neutralizing agent is triethylamine.
[0071] The amount of the neutralizer used is preferably 1 to 4 parts by weight; more preferably 1.5 to 2 parts by weight.
[0072] The reaction temperature of this step may be 50 to 75° C., preferably 55 to 70° C., and more preferably 60 to 65° C. The reaction time may be 0.5 to 4 h, preferably 1 to 3 h, and more preferably 2 to 2.5 h.
[0073] Specifically, a primary prepolymer having a temperature of ≤50° C., a hydrophilic chain extender and a neutralizer are mixed. Preferably, the temperature of the primary prepolymer is ≤40° C. More preferably, the temperature of the primary prepolymer is 20-40° C.
[0074] <Step of Obtaining Emulsified Product>
[0075] The secondary prepolymer is emulsified in the presence of an emulsifier, and then water is added for further emulsification to obtain an emulsified product. In certain embodiments, the secondary prepolymer is directly emulsified with the emulsifier without cooling.
[0076] In the present invention, the emulsifier includes water and sodium fatty alcohol polyoxyethylene ether carboxylate. In certain embodiments, the emulsifier consists of water and sodium fatty alcohol polyoxyethylene ether carboxylate. The amount of water can be 15 to 45 parts by weight; preferably 20 to 40 parts by weight; more preferably 30 to 35 parts by weight. The amount of sodium fatty alcohol polyoxyethylene ether carboxylate can be 0.5 to 3 parts by weight; preferably 1 to 2.5 parts by weight; more preferably 1.5 to 2 parts by weight.
[0077] The emulsification time of the secondary prepolymer and the emulsifier is 1 to 10 minutes, preferably 2 to 8 minutes, and more preferably 5 to 6 minutes.
[0078] In the present invention, water is added to the intermediate emulsion obtained by emulsifying the secondary prepolymer and the emulsifier for further emulsification to obtain an emulsified product.
[0079] The amount of water added to the intermediate emulsion may be 40 to 75 parts by weight, preferably 45 to 65 parts by weight, and more preferably 55 to 60 parts by weight.
[0080] The further emulsification can be carried out at a temperature of 15 to 35°C, preferably 20 to 30°C.
[0081] The time for further emulsification may be 5 to 20 minutes, preferably 8 to 15 minutes, and more preferably 10 to 12 minutes.
[0082] In certain embodiments, water is added to the intermediate emulsion at a temperature of 15 to 35°C, preferably 20 to 30°C, and more preferably 20 to 25°C for further emulsification.
[0083] <Step of Obtaining Polyurethane Emulsion>
[0084] The emulsified product, 2 to 8 parts by weight of isophorone diamine and 1 to 5 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane are reacted to obtain a polyurethane emulsion.
[0085] The amount of isophorone diamine used is preferably 4 to 7 parts by weight; more preferably 5 to 6 parts by weight.
[0086] The amount of N-2-aminoethyl-3-aminopropyltriethoxysilane used is preferably 2 to 4 parts by weight; more preferably 2.5 to 3 parts by weight.
[0087] The reaction temperature may be 15 to 35°C; preferably 20 to 30°C; more preferably 20 to 25°C.
[0088] The reaction time may be 0.4 to 5 h; preferably 1 to 3 h; more preferably 1 to 2 h.
[0089] The solid content of the polyurethane emulsion is ≥45 wt %, preferably ≥50 wt %. In certain embodiments, the solid content is 55-60 wt %.
[0090] The viscosity of the polyurethane emulsion is ≤700 cP; preferably, the viscosity is ≤680 cP. In certain embodiments, the viscosity of the polyurethane emulsion is 650-670 cP.
[0091] The tensile strength of the polyurethane emulsion after curing is ≥50 MPa; preferably, the tensile strength is ≥55 MPa. In some embodiments, the tensile strength is 56-60 MPa.
[0092] The bonding strength of the polyurethane emulsion after curing is ≥55N; preferably, the bonding strength is ≥60N. In some embodiments, the bonding strength is 62-65N.
[0093] The elongation of the polyurethane emulsion after curing is ≥600%; preferably, the elongation is ≥630%; more preferably, the elongation is 640-650%.
[0094] The 100% tensile strength of the polyurethane emulsion after curing is 5 to 15 MPa. In certain embodiments, the 100% tensile strength is 10 to 12 MPa.
[0095] The polyurethane emulsion of the invention has good solvent resistance after film formation and is insoluble in tetrahydrofuran.
[0096] Here are the raw materials:
[0097] The brand name of sodium fatty alcohol polyoxyethylene ether carboxylate is: AEC-9Na, and the manufacturer is: Jining Fangyu Chemical Co., Ltd.
[0098] The molecular weight of polypropylene glycol is 2000.
[0099] The molecular weight of polybutylene adipate diol is 3,000.
[0100] Example 1
[0101] (1) 25 parts by weight of polypropylene glycol and 40 parts by weight of polybutylene adipate diol were dehydrated at 120° C. in vacuum for 2 h to obtain dehydrated polypropylene glycol and dehydrated polybutylene adipate diol.
[0102] (2) The dehydrated polypropylene glycol and the dehydrated polybutylene adipate diol are cooled to 60° C. under the protection of nitrogen, and then 10 parts by weight of hexamethylene diisocyanate, 17 parts by weight of 4,4'-diisocyanate dicyclohexylmethane and 0.08 parts by weight of bismuth isooctanoate are added to the dehydrated polypropylene glycol and the dehydrated polybutylene adipate diol. After the above raw materials are mixed evenly, the mixture is reacted at 85° C. for 3 hours under stirring to obtain a primary prepolymer.
[0103] (3) The primary prepolymer at 40° C., 7 parts by weight of dimethylolbutyric acid and 1.7 parts by weight of triethylamine were mixed and then reacted at 60° C. for 2 hours to obtain a secondary prepolymer.
[0104] (4) Add an emulsifier to the secondary prepolymer and emulsify for 5 minutes to obtain an intermediate emulsion. The intermediate emulsion is cooled to 25° C., and then 57 parts by weight of deionized water is added and further emulsified for 10 minutes to obtain an emulsified product. The emulsifier is composed of 30 parts by weight of deionized water and 1.8 parts by weight of sodium fatty alcohol polyoxyethylene ether carboxylate.
[0105] (5) The emulsified product, 6 parts by weight of isophorone diamine and 2.7 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane were reacted at 25° C. for 1 hour to obtain a polyurethane emulsion.
[0106] Comparative Example 1
[0107] Except that isophorone diamine is replaced by 1,4-butanediol, the rest is the same as Example 1.
[0108] Comparative Example 2
[0109] The same procedures as in Example 1 were followed except that 6 parts by weight of isophorone diamine and 2.7 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane in step (5) were replaced by 8.7 parts by weight of isophorone diamine.
[0110] Comparative Example 3
[0111] Except that the emulsifier in step (4) is replaced by 30 parts by weight of deionized water, the rest is the same as Example 1.
[0112] Comparative Example 4
[0113] (1) 25 parts by weight of polypropylene glycol and 40 parts by weight of polybutylene adipate diol were dehydrated at 120° C. in vacuum for 2 h to obtain dehydrated polypropylene glycol and dehydrated polybutylene adipate diol.
[0114] (2) The dehydrated polypropylene glycol and the dehydrated polybutylene adipate diol are cooled to 60° C. under the protection of nitrogen, and then 10 parts by weight of hexamethylene diisocyanate, 17 parts by weight of 4,4'-diisocyanate dicyclohexylmethane and 0.08 parts by weight of bismuth isooctanoate are added to the dehydrated polypropylene glycol and the dehydrated polybutylene adipate diol. After the above raw materials are mixed evenly, the mixture is reacted at 85° C. for 3 hours under stirring to obtain a primary prepolymer.
[0115] (3) The primary prepolymer at 70° C., 7 parts by weight of dimethylolbutyric acid and 30 parts by weight of butanone were reacted at 70° C. for 2 hours to obtain a secondary prepolymer.
[0116] (4) After the secondary prepolymer was cooled to 40° C., 1.7 parts by weight of triethylamine and 87 parts by weight of deionized water were added to the secondary prepolymer and emulsified for 20 minutes to obtain an emulsified product.
[0117] (5) The emulsified product was cooled to 25° C., and then 6 parts by weight of isophorone diamine and 2.7 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane were added to the emulsified product for reaction for 1 hour to obtain a reaction product. The butanone in the reaction product was distilled under reduced pressure to obtain a polyurethane emulsion.
[0118] Experimental example
[0119] The performance of the polyurethane emulsion was tested using the following method, and the results are shown in Table 1:
[0120] Solid content: According to BS EN ISO 3251-2019 Paints, varnishes and plastics - Determination of non-volatile matter content.
[0121] Viscosity: The melt viscosity at 25°C was measured using a Brookfield DV2T rotational viscometer.
[0122] Tensile strength: measured according to the method specified in GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.
[0123] Elongation: measured according to the method specified in GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.
[0124] 100% modulus of tensile strength: measured according to the method specified in GB / T528-2009 Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber.
[0125] Adhesive strength: According to the method specified in GJB-446-1988 Adhesive 90° Peel Strength Test Method.
[0126] Solvent resistance: The polyurethane emulsion was cured into a film and cut into square specimens of 50 mm × 50 mm. The specimens were placed in THF solvent and the dissolution of the specimens was observed after 6 hours.
[0127] Table 1
[0128]
[0129] It can be seen from Example 1 and Comparative Examples 1-2 that the type and amount of the chain extender used in step (5) have an important influence on the mechanical properties, bonding strength and solvent resistance of the polyurethane emulsion after film formation. The tensile strength, 100% tensile strength and bonding strength of the polyurethane emulsions of Comparative Examples 1 and 2 after film formation are significantly lower than those of Example 1, and the solvent resistance of the polyurethane emulsions of Comparative Examples 1 and 2 after film formation is poor.
[0130] It can be seen from Example 1 and Comparative Example 3 that the addition of sodium fatty alcohol polyoxyethylene ether carboxylate can improve the stability and uniformity of the polyurethane emulsion, and can improve the mechanical properties and bonding strength of the polyurethane emulsion after film formation.
[0131] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for preparing a polyurethane emulsion, characterized in that: The steps include: (1) removing water from 15 to 35 parts by weight of polypropylene glycol and 30 to 50 parts by weight of polybutylene adipate diol to obtain dehydrated polypropylene glycol and dehydrated polybutylene adipate diol; (2) reacting the dehydrated polypropylene glycol, the dehydrated polybutylene adipate glycol, 5 to 15 parts by weight of a first diisocyanate, 12 to 25 parts by weight of a second diisocyanate, and 0.03 to 0.2 parts by weight of an organic bismuth catalyst to obtain a primary prepolymer; Wherein, the first diisocyanate is as shown in formula (A): In formula (A), m is an integer selected from 1 to 8; Wherein, the second diisocyanate is as shown in formula (B): In formula (B), R1 is selected from C1-C6 alkylene, and R2-R9 are independently selected from H or C1-C6 alkyl; (3) mixing a primary prepolymer at a temperature of ≤45° C., 2 to 15 parts by weight of a hydrophilic chain extender, and 0.5 to 3 parts by weight of a neutralizer, and reacting the mixture at 50 to 75° C. for 0.5 to 4 hours to obtain a secondary prepolymer; (4) emulsifying the secondary prepolymer in the presence of an emulsifier, and then adding water for further emulsification to obtain an emulsified product; the emulsifier includes water and sodium fatty alcohol polyoxyethylene ether carboxylate; (5) The emulsified product, 2 to 8 parts by weight of isophorone diamine and 1 to 5 parts by weight of N-2-aminoethyl-3-aminopropyltriethoxysilane are reacted to obtain a polyurethane emulsion.
2. The preparation method according to claim 1, characterized in that: In formula (A), m is selected from an integer of 2 to 6; in formula (B), R1 is selected from a C1 to C3 alkylene group, and R2 to R9 are independently selected from H or a C1 to C3 alkyl group; the organic bismuth catalyst is selected from one or more of bismuth neodecanoate, bismuth isooctanoate, and bismuth laurate.
3. The preparation method according to claim 1, characterized in that: The first diisocyanate is hexamethylene diisocyanate, and the second diisocyanate is 4,4'-diisocyanate dicyclohexylmethane.
4. The preparation method according to claim 1, characterized in that: In step (2), the polypropylene glycol after dehydration at a temperature of ≤70°C, the polybutylene adipate diol after dehydration at a temperature of ≤70°C, the first diisocyanate, the second diisocyanate and the organic bismuth catalyst are mixed, and then reacted at 70-95°C for 1-10 hours under stirring.
5. The preparation method according to claim 1, characterized in that: The hydrophilic chain extender is shown in formula (C): In formula (C), R 10 and R 11 are independently selected from C1 to C6 alkylene groups, and Q is selected from an integer of 1 to 6; The neutralizing agent is selected from one or more of triethylamine, tripropylamine, tributylamine, dimethylcyclohexylamine, formic acid, acetic acid, hydrochloric acid, sodium hydroxide, and epichlorohydrin.
6. The preparation method according to claim 1, characterized in that: In the emulsifier, water accounts for 15 to 45 parts by weight, and sodium fatty alcohol polyoxyethylene ether carboxylate accounts for 0.5 to 3 parts by weight.
7. The preparation method according to claim 1, characterized in that: In step (4), the secondary prepolymer is emulsified in the presence of an emulsifier for 1 to 10 minutes, and then 40 to 75 parts by weight of water are added and further emulsified for 5 to 20 minutes.
8. The preparation method according to claim 1, characterized in that: In step (5), the reaction temperature is 15 to 38° C. and the reaction time is 0.5 to 3 h.
9. The preparation method according to any one of claims 1 to 8, characterized in that: The polyurethane emulsion has a solid content of ≥45wt% and a viscosity of ≤700cP.