A method for preparing polyester from alkylene oxide and cyclic anhydride

By using N,N,N-trimethyl-N'-N''-(2-aminoethyl)-1,2-ethylenediamine bridged tris(2-hydroxy-3,5-di-tert-butyl phenyl) quaternary ammonium salt catalyzes the copolymerization of alkylene oxide and cyclic acid anhydride, solving the problems of metal residue and harsh reaction conditions, achieving highly selective and highly active polyester preparation, and is suitable for biomedicine and food fields .

CN118165241BActive Publication Date: 2024-10-01SUZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410592934.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-14
Publication Date
2024-10-01
Estimated Expiration
2044-05-14

AI Technical Summary

Technical Problem

In the ring-opening copolymerization of alkylene oxide and cyclic anhydride, the problem of metal residue caused by metal catalysts hinders the application of polyester in the fields of biomedicine and food, and traditional methods have harsh reaction conditions or high costs, and low atom economy.

Method used

Using N,N,N-trimethyl-N'-N''-(2-aminoethyl)-1,2-ethylenediamine bridged tris(2-hydroxy-3,5-di-tert-butyl) Phenyl) quaternary ammonium salt is used as a catalyst to catalyze the copolymerization of alkylene oxide and cyclic acid anhydride at 80-120°C to form a highly selective and highly active polyester.

Benefits of technology

It achieves no metal ion residue, high catalytic activity, mild reaction conditions, acid anhydride conversion rate up to 91%, polyester selectivity up to 99%, and has broad application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118165241B_ABST
    Figure CN118165241B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of small molecule copolymerization, and in particular to a method for preparing polyester using alkylene oxide and cyclic anhydride as raw materials. The present invention discloses a method for preparing polyester from alkylene oxide and cyclic anhydride, wherein the method uses triphenol functionalized quaternary ammonium salt as a catalyst, and catalyzes copolymerization of alkylene oxide and cyclic anhydride under heating conditions of 80-120°C in an organic solvent to form a polymer. These quaternary ammonium salts have high catalytic activity, and can enable cyclic anhydride to be completely converted in a polymerization reaction, and the polyester selectivity in the obtained polymer can be greater than 99%. The method has the advantages of simple reaction operation, high yield and selectivity of the obtained polymer, and the obtained polymer avoids the problem of metal residues existing in previous metal catalysts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of small molecule copolymerization, and particularly relates to a method for preparing polyester from alkylene oxide and cyclic acid anhydride. Background Art

[0002] Polyester is a biodegradable polymer material that is widely used in daily necessities, medical equipment and other fields. In the traditional method of preparing polyester, on the one hand, polyester is prepared by condensation reaction of diols and dibasic acids. The reaction conditions are harsh and small molecules are continuously removed during the polymerization process, resulting in low atom economy. On the other hand, polymers are formed by ring-opening polymerization of lactones. This method has good atom economy and the reaction is relatively mild and controllable, but the preparation cost of the reaction monomer is relatively high, the synthesis steps are relatively complex and the types are limited. In contrast, the preparation of polyester by alternating ring-opening copolymerization (ROCOP) of alkylene oxide and cyclic anhydride has good atom economy, and the reaction monomers are rich in variety, cheap and easy to obtain. Polyesters with different structures can be prepared by combining different anhydrides with alkylene oxides, so that the properties of the resulting polyester can be adjusted more flexibly. Therefore, the ring-opening copolymerization of alkylene oxide and cyclic anhydride has received widespread attention in recent years.

[0003] There are two catalytic systems in the ring-opening copolymerization of alkylene oxide and cyclic anhydride: metal catalytic system and organic catalytic system, among which the metal complex catalytic system started earlier. It has been reported in the literature that metal complexes such as zinc, manganese, aluminum, chromium and cobalt can catalyze the ring-opening copolymerization of alkylene oxide and cyclic anhydride, and can effectively inhibit the isomerization, transesterification and homopolymerization of alkylene oxide during the polymerization process, which has promoted the production of industrial polyester (reference: Longo, JM, Sanford, MJ, Coates, GW, Chem. Rev. 2016, 116 , 24, 15167-15197.). However, in the system where metal complexes are used as catalysts, the problem of metal residues in the resulting polymers is difficult to solve, which hinders the application of polyesters in the fields of biomedicine, food, etc.

[0004] In recent years, in order to avoid the problem of metal residues on polymers, the application of organic catalytic systems in the copolymerization of cyclic anhydrides and alkylene oxides has gradually attracted people's attention. In 2017, a foreign research group reported that organic bases such as dimethylaminopyridine (DMAP), bis(triphenylphosphine) ammonium chloride (PPNCl), and triphenylphosphine (PPh3) can catalyze the ring-opening copolymerization of phthalic anhydride (PA) and cyclohexane oxide (CHO) in a 110 °C toluene solution to obtain alternating copolymerized polyesters. Among them, the most effective catalyst is bis(triphenylphosphine) ammonium chloride (PPNCl). When reacted at 110 °C for 10 h, the conversion rate of alkylene oxide can reach 90%, and the molecular weight distribution of the resulting polyester is narrow. , but there are 2% polyether chains in the resulting polymer (reference: Eur. Polym. J. 2017, 88 , 433-447.).

[0005] In 2021, Wu Guangpeng's research group screened a series of organoboron compounds for catalytic copolymerization of alkylene oxide and cyclic anhydride. When the reaction temperature was 180 °C, the TOF value could reach up to 915 h -1 By optimizing the reaction conditions of ring-opening polymerization, polyester with narrow molecular weight distribution (1.10-1.40) and average molecular weight up to 94.5 kDa can be obtained (Reference: Xie, R., Zhang, YY, Yang, GW, Zhu, XF, Li, B., Wu, GP, Angew. Chem. Int. Oath. 2021, 60 , 19253-19261.).

[0006] It can be seen that organic catalysts have great development potential for catalyzing the copolymerization of cyclic anhydrides and alkylene oxides. It is very meaningful to develop low-cost and efficient organic catalysts that can catalyze the copolymerization of alkylene oxides and cyclic anhydrides to form highly selective polyesters under relatively mild conditions. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a method for preparing polyester using organic compounds as catalysts. N , N , N -Trimethyl- N '- N''-(2-aminoethyl)-1,2-ethylenediamine bridged tri(2-hydroxy-3,5-di-tert-butylphenyl) quaternary ammonium salt is used as a catalyst to catalyze the copolymerization of alkylene oxide and cyclic anhydride to form polyester at 80-120 ℃. The reaction conditions of this system are relatively mild, the catalytic activity of the catalyst used is high, and the selectivity of polyester in the resulting polymer is good. At 100 ℃, using toluene as a solvent for one hour, epichlorohydrin and phthalic anhydride are catalyzed to copolymerize into poly(chloropropyl phthalate), the conversion rate of anhydride is as high as 91%, and the selectivity of polyester in the resulting product is as high as 99%, which has great potential application value.

[0008] In order to solve the above-mentioned technical problems, this application provides the following technical solutions:

[0009] The present invention discloses a method for preparing polyester (Formula I) from alkylene oxide and cyclic anhydride, wherein the method uses triphenol functionalized quaternary ammonium salt (Formula II) as a catalyst, and catalyzes copolymerization of alkylene oxide and cyclic anhydride under heating conditions of 80-120° C. in an organic solvent to form a polymer. These quaternary ammonium salts have high catalytic activity, can achieve complete conversion of cyclic anhydride in the polymerization reaction, and the polyester selectivity in the obtained polymer can be as high as greater than 99%.

[0010] ;

[0011] Wherein, R1 is a hydrogen atom; R2 is one of methyl, chloromethylene, and ethyl; X - Chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) or methanesulfonate ion (MeSO3 - ).

[0012] The present invention provides a method for preparing polyester from alkylene oxide and cyclic acid anhydride, comprising the following steps:

[0013] Cyclic anhydride, alkylene oxide and catalyst are mixed in an organic solvent and heated to react to obtain highly selective polyester;

[0014] The catalyst is selected from triphenol functionalized quaternary ammonium salt.

[0015] Preferably, the triphenol functionalized quaternary ammonium salt is selected from N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl) quaternary ammonium salt, whose structural formula is as shown in (Formula III).

[0016] ;

[0017] Among them, X - One selected from chloride ion, bromide ion, iodide ion or methanesulfonate ion.

[0018] Preferably, the molar ratio of the catalyst to the cyclic anhydride is 1:50-200.

[0019] Preferably, the molar ratio of the catalyst to the alkylene oxide is 1:100-400.

[0020] Preferably, the organic solvent is toluene, hexane or cyclohexane.

[0021] Preferably, the temperature of the heating reaction is 80-120°C.

[0022] Furthermore, the temperature of the heating reaction is specifically any value between two numerical values.

[0023] Preferably, the heating reaction time is 1-6 h.

[0024] Furthermore, the time of the heating reaction is specifically any value between two numerical values.

[0025] Preferably, the cyclic anhydride is selected from one of phthalic anhydride (PA), maleic anhydride (MA), succinic anhydride (SA) and glutaric anhydride (GA).

[0026] Preferably, the alkylene oxide is one of epichlorohydrin (ECH), propylene oxide (PO) and butylene oxide (BO).

[0027] The present invention also provides a highly selective polyester prepared by the above method for preparing polyester from alkylene oxide and cyclic acid anhydride.

[0028] The technical solution of the present invention has the following advantages over the prior art:

[0029] The invention discloses an application of a simple and readily available triphenol functionalized quaternary ammonium salt in catalyzing the copolymerization of alkylene oxide and cyclic acid anhydride to obtain polyester. The system has the advantages that the catalyst is organic and does not contain metal ions, thereby avoiding the residual metal ions in the obtained polymer; the catalyst used has high activity; the reaction conditions are mild; the acid anhydride conversion rate and the selectivity of polyester in the obtained polymer are high.

[0030] In the present invention, under heating conditions, the catalyst catalyzes the copolymerization of alkylene oxide and cyclic anhydride. After the reaction is completed, dichloromethane is used to quench the reaction and dissolve the product. Ethanol is added to precipitate the polymer, which is filtered and dried to obtain a white polymer. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1For poly(ECH- all -PA) MALDI-TOF mass spectrometry (MS) spectrum; where m / z = 240.64*n(ECH- all -PA) + 22.99 (Na + ) + 95.13 (MeSO3 - ) + 1.01 (H + ). DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0033] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.

[0034] Example 1

[0035] This embodiment provides N , N , N -Trimethyl- N '- N Phthalic anhydride and epichlorohydrin (molar ratio of catalyst [Cat.]: phthalic anhydride [PA]: epichlorohydrin [ECH] = 1:50:100) were copolymerized at 80 ℃ by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0036] First, use a pipette to measure 0.20 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene and add them to a pressure bottle. Then use an analytical balance to weigh 0.185 g (1.25 mmol) of phthalic anhydride and the catalyst. N , N , N -Trimethyl- N '- N22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 80 °C for 4 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be 82%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.4 kDa, and the molecular weight distribution was 1.50.

[0037] Example 2

[0038] This embodiment provides N , N , N -Trimethyl- N '- N The copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] = 1:50:100) at 80 ℃ was catalyzed by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0039] First, 0.20 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.185 g of phthalic anhydride (1.25 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 80 °C for 5 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be greater than 99%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.8 kDa and the molecular weight distribution was 1.40.

[0040] Example 3

[0041] This embodiment provides N , N , N -Trimethyl- N '- N The copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] = 1:50:100) at 70 ℃ was catalyzed by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0042] First, 0.20 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of n-hexane were added to a pressure bottle, and then 0.185 g of phthalic anhydride (1.25 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 70 °C for 5 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization. The conversion rate of phthalic anhydride was measured to be 68%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.5 kDa and the molecular weight distribution was 1.45.

[0043] Example 4

[0044] This embodiment provides N , N , N -Trimethyl- N '- N Phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] = 1:50:100) were copolymerized at 100 ℃ by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzed to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0045] First, 0.20 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.185 g of phthalic anhydride (1.25 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 3 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be greater than 99%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 4.7 kDa, and the molecular weight distribution was 1.39.

[0046] Example 5

[0047] This embodiment provides N , N , N -Trimethyl- N '- N Phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] = 1:50:100) were copolymerized at 100 ℃ by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzed to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0048] First, 0.20 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.185 g of phthalic anhydride (1.25 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 1 hour. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization. The conversion rate of phthalic anhydride was measured to be 91%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 4.3 kDa, and the molecular weight distribution was 1.26.

[0049] Example 6

[0050] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzes the copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] = 1:100:100) at 100 ℃ to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0051] First, 0.39 mL of epichlorohydrin (5 mmol) and 0.5 mL of toluene were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 44.8 mg (0.05 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 1 hour. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be 63%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 2.3 kDa, and the molecular weight distribution was 1.26.

[0052] Example 7

[0053] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)ammonium chloride catalyzes the copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] =1:100:100) at 100 ℃ to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0054] First, 0.39 mL of epichlorohydrin (5 mmol) and 0.5 mL of toluene were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N,N,N -Trimethyl- N '- N 41.8 mg (0.05 mmol) of ''-(2-aminoethyl)-1, 2-ethylenediamine-bridged tri(2-hydroxy-3, 5-di-tert-butylphenyl)ammonium chloride was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 1 hour. After the reaction, the pressure bottle was removed, and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be 29%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer. Dry. The polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 2.1 kDa, and the molecular weight distribution was 1.18.

[0055] Example 8

[0056] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)ammonium bromide catalyzes the copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] =1:100:100) at 100 ℃ to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0057] First, 0.39 mL of epichlorohydrin (5 mmol) and 0.5 mL of toluene were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 44.0 mg (0.05 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)ammonium bromide was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 1 hour. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be 60%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.8 kDa, and the molecular weight distribution was 1.16.

[0058] Example 9

[0059] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)ammonium iodide catalyzes the copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] =1:100:100) at 100 ℃ to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0060] First, 0.39 mL of epichlorohydrin (5 mmol) and 0.5 mL of toluene were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N46.4 mg (0.05 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)ammonium iodide was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for reaction for 1 hour. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be 39%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.9 kDa, and the molecular weight distribution was 1.19.

[0061] Example 10

[0062] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzes the copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] =1:100:200) at 100 ℃ to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0063] First, 0.39 mL of epichlorohydrin (5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.37 g of phthalic anhydride (2.5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 4 hours. After the reaction, the pressure bottle was removed, and a small amount of the reaction solution was taken for nuclear magnetic resonance hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be greater than 99%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic resonance hydrogen spectrum, and the selectivity of polyester in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 5.3 kDa, and the molecular weight distribution was 1.35. The polymer was characterized by matrix-assisted laser desorption ionization time-of-flight (MALDI-TOF) mass spectrometry (such as Figure 1 As shown), it shows that the obtained polymers are all polymers of complete alternating copolymerization of phthalic anhydride and epichlorohydrin monomers initiated by methanesulfonic acid anions.

[0064] Embodiment 11

[0065] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzes the copolymerization of phthalic anhydride and epichlorohydrin ([Cat.]:[PA]:[ECH] =1:200:400) at 100 ℃ to form poly(chloropropyl phthalate) poly(ECH- all -PA).

[0066] First, 0.78 mL of epichlorohydrin (10 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 6 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be greater than 99%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 6.1 kDa, and the molecular weight distribution was 1.40.

[0067] Example 12

[0068] This embodiment provides N , N , N -Trimethyl- N '- N''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzes the copolymerization of phthalic anhydride and propylene oxide ([Cat.]:[PA]:[PO]=1:200:200) at 80 ℃ to form poly(propyl phthalate) poly(PO- all -PA).

[0069] First, 0.31 mL of propylene oxide (5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 80 °C for 8 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization. The conversion rate of phthalic anhydride was measured to be 78%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be 82%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.7 kDa, and the molecular weight distribution was 1.15.

[0070] Embodiment 13

[0071] This embodiment provides N , N , N -Trimethyl- N '- N The copolymerization of phthalic anhydride and propylene oxide ([Cat.]:[PA]:[PO]=1:200:200) at 80 ℃ was catalyzed by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium to form poly(ECH- all -PA).

[0072] First, 0.31 mL of propylene oxide (5 mmol) and 0.25 mL of cyclohexane were added to a pressure bottle, and then 0.74 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '-N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 80 °C for 8 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of phthalic anhydride was measured to be 80%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be 78%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 1.9 kDa, and the molecular weight distribution was 1.17.

[0073] Embodiment 14

[0074] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzes the copolymerization of maleic anhydride and epichlorohydrin ([Cat.]:[MA]:[ECH] =1:50:100) at 100 ℃ to form poly(chloropropyl maleate) poly(ECH- all -MA).

[0075] First, 0.2 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.123 g of maleic anhydride (1.25 mmol) and catalyst were weighed on an analytical balance. N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 1 hour. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the maleic anhydride conversion rate was measured to be 70%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 2.1 kDa, and the molecular weight distribution was 1.25.

[0076] Embodiment 15

[0077] This embodiment provides N , N ,N -Trimethyl- N '- N Succinic anhydride and epichlorohydrin ([Cat.]:[SA]:[ECH] =1:50:100) were copolymerized at 100 ℃ by ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzed to form poly(ECH- all -SA).

[0078] First, 0.2 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.125 g of succinic anhydride (1.25 mmol) and the catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 6 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of succinic anhydride was measured to be greater than 99%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 2.2 kDa, and the molecular weight distribution was 1.64.

[0079] Example 16

[0080] This embodiment provides N , N , N -Trimethyl- N '- N Glutaric anhydride and epichlorohydrin ([Cat.]:[GA]:[ECH] =1:50:100) were copolymerized at 100 ℃ by tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate bridged by ''-(2-aminoethyl)-1,2-ethylenediamine to form poly(ECH- all -GA).

[0081] First, 0.39 mL of epichlorohydrin (2.5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.143 g of glutaric anhydride (1.25 mmol) and catalyst were weighed on an analytical balance. N ,N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 100 °C for 4 hours. After the reaction, the pressure bottle was removed and a small amount of the reaction solution was taken for nuclear magnetic hydrogen spectrum characterization, and the conversion rate of glutaric anhydride was measured to be 83%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 3.2 kDa, and the molecular weight distribution was 1.53.

[0082] Embodiment 17

[0083] This embodiment provides N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium catalyzes the copolymerization of phthalic anhydride and butylene oxide ([Cat.]:[PA]:[BO]=1:200:200) at 120 ℃ to form polybutylene phthalate poly(BO- all -PA).

[0084] First, 0.44 mL of butylene oxide (5 mmol) and 0.25 mL of toluene were added to a pressure bottle, and then 0.729 g of phthalic anhydride (5 mmol) and catalyst were weighed on an analytical balance. N , N , N -Trimethyl- N '- N 22.4 mg (0.025 mmol) of ''-(2-aminoethyl)-1,2-ethylenediamine-bridged tri(2-hydroxy-3,5-di-tert-butylphenyl)methanesulfonate ammonium was added to the same pressure bottle. Then, the pressure bottle was placed in an oil bath at 120 °C for 5 hours. After the reaction, the pressure bottle was removed, a small amount of the reaction solution was taken, and nuclear magnetic hydrogen spectrum was characterized, and the conversion rate of phthalic anhydride was measured to be greater than 99%. Dichloromethane was then added to the reaction system to quench the reaction, and then ethanol was added to precipitate the polymer and dry it. The obtained polymer was characterized by nuclear magnetic hydrogen spectrum, and the polyester selectivity in the polymer was measured to be greater than 99%. The number average molecular weight of the polymer was measured by gel permeation chromatography to be 3.5 kDa, and the molecular weight distribution was 1.13.

[0085] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A method for preparing polyester from alkylene oxide and cyclic anhydride, It is characterized in that The following steps are involved: Cyclic anhydride, alkylene oxide and catalyst are mixed in an organic solvent, and ring-opening polymerization is carried out at 80-120°C to obtain highly selective polyester; the catalyst is selected from triphenol functionalized quaternary ammonium salt; the triphenol functionalized quaternary ammonium salt is selected from N , N , N -Trimethyl- N '- N ''-(2-aminoethyl)-1,2-ethylenediamine bridged tris(2-hydroxy-3,5-di-tert-butylphenyl) quaternary ammonium salt, the structural formula of which is as follows: ; Among them, X - Selected from chloride, bromide, iodide or methanesulfonate ions.

2. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The molar ratio of the catalyst to the cyclic anhydride is 1:50-200.

3. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The molar ratio of the catalyst to the alkylene oxide is 1:100-400.

4. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The organic solvent is toluene, n-hexane or cyclohexane.

5. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The temperature of the ring-opening polymerization reaction is 80-120°C.

6. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The ring-opening polymerization reaction time is 1-6 h.

7. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The cyclic anhydride is selected from one of phthalic anhydride, maleic anhydride, succinic anhydride and glutaric anhydride.

8. A method for preparing polyester from alkylene oxide and cyclic anhydride as claimed in claim 1, It is characterized in that The alkylene oxide is one of epichlorohydrin, propylene oxide and butylene oxide.

Citation Information

Patent Citations

  • Method for preparing polyester from (thio)urea / organic alkali catalyzed epoxides and cyclic anhydrides by ring-opening copolymerization

    CN109679077A

  • Heteronuclear metal complex and preparation method of cyclic carbonate catalyzed by heteronuclear metal complex

    CN109705172A

  • Aliphatic-aromatic copolyester and preparation method thereof

    CN110256657A

  • Catalysts for the oxirane-anhydride reaction

    US3977996A