Self-repairing flame retardant coating and preparation method thereof
By combining acrylate copolymers with modified nano-concave and concave rock stones in the coating, a thermally reversible crosslinking network is formed and fluorine atoms and DOPO structures are introduced, which solves the problems of flammable and incapable of self-repair in traditional coatings and realizes self-repair and the improvement of flame retardant performance reduces fire risk and extends service life.
Patent Information
- Application Number
- CN202410335813.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-22
AI Technical Summary
Traditional coatings are flammable during production and use and cannot be self-repaired, resulting in a decrease in fire risk and service life, which cannot meet the increasingly stringent performance needs.
Acrylate copolymer is combined with modified nano-concave and concave rock stone, and a thermally reversible crosslinking network is formed through Diels-Alder addition reaction, combining fluorine atoms and DOPO structures to prepare a coating with self-healing and flame retardant properties.
It has achieved improvements in the self-repairing performance and flame retardant performance of the coating, extended service life, reduced fire risk, and improved corrosion resistance.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer materials, and in particular to a self-repairing flame-retardant coating and a preparation method thereof. Background Art
[0002] Paint is a viscous liquid coated on the surface of an object to be protected or decorated, and can form a firmly attached continuous film with the coated object. It is usually mainly resin, oil or emulsion, with or without pigments, fillers, and corresponding additives, and is prepared with organic solvents or water. Paint is widely used in many fields such as construction, food packaging, transportation, health care, and electronic products. With the development of the economy and the advancement of science and technology, people have put forward new requirements for the performance of paint in production and life, and traditional paint preparation processes and technologies are difficult to meet the ever-changing needs. For example, the raw materials for preparing paints are mostly polymer materials, which are very easy to burn and cause fires during production and use, causing casualties and economic losses; paints cannot automatically recover after being damaged, which reduces their service life and increases costs. Therefore, the development of a paint with self-healing and flame-retardant properties has important practical significance and broad development prospects. Summary of the invention
[0003] The purpose of the present invention is to provide a self-repairing flame retardant coating and a preparation method thereof to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A self-repairing flame-retardant coating, wherein the self-repairing flame-retardant coating is prepared by reacting methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate and allyl anthracene monomers to obtain an acrylate copolymer emulsion; reacting nano-attapulgite with 3-isocyanatopropyltriethoxysilane, modified DOPO and 3-maleimide propionic acid in sequence to obtain modified nano-attapulgite; and uniformly mixing the acrylate copolymer emulsion, the modified nano-attapulgite and a defoamer.
[0006] As an optimization, the allyl anthracene monomer is prepared by reacting allyl glycidyl ether with 9-anthracenecarboxylic acid.
[0007] As an optimization, the modified DOPO is prepared by reacting diethanolamine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0008] A method for preparing a self-repairing flame retardant coating comprises the following preparation steps:
[0009] (1) adding allyl glycidyl ether and 9-anthracenecarboxylic acid in a molar ratio of 1:1 to tetrahydrofuran (18 to 20 times the mass of allyl glycidyl ether), stirring at 60 to 64°C and 300 to 500 r / min for 20 to 24 hours, and drying at 5 to 7 Pa and 50 to 60°C for 6 to 7 hours to obtain allyl anthracene monomer;
[0010] (2) Methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate, and allyl anthracene monomers are mixed at a mass ratio of 1:1:(0.1~0.2):(0.1~0.2) to prepare a mixed monomer; potassium persulfate (0.01~0.03 times the mass of the mixed monomer) and deionized water are mixed at a mass ratio of 1:(20~30) to prepare a potassium persulfate aqueous solution; polyether nonionic emulsifier (0.05~0.07 times the mass of the mixed monomer) and deionized water are mixed at a mass ratio of 1:(180~200) to prepare a mixed monomer solution; , raise the temperature to 70-80°C, uniformly add 8-10% of the total amount of the mixed monomers and 8-10% of the total amount of the potassium persulfate aqueous solution within 10 minutes, stir and react at 70-80°C, 300-500r / min for 15-17 minutes to obtain a seed emulsion; uniformly add the remaining mixed monomers and the potassium persulfate aqueous solution to the seed emulsion within 2-3 hours, stir and react at 80-90°C, 300-500r / min for 40-50 minutes, cool to room temperature, filter, and obtain an acrylate copolymer emulsion;
[0011] (3) Add diethanolamine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and triethylamine in a molar ratio of 1:1:1 to dichloromethane (8 to 10 times the mass of diethanolamine), cool to -10 to 0°C, and under a nitrogen atmosphere, add carbon tetrachloride (0.04 to 0.06 times the mass of diethanolamine) dropwise at a constant rate within 10 minutes at a stirring rate of 300 to 500 r / min. Continue stirring and reacting for 20 to 24 hours, filter, and wash the filtrate with a sodium bicarbonate aqueous solution (8 to 10% by mass) and a saturated sodium chloride aqueous solution (3 to 5 times each), and dry at 5 to 7 Pa and 40 to 50°C for 6 to 7 hours to obtain modified DOPO;
[0012] (4) 3-isocyanatopropyltriethoxysilane and deionized water were mixed at a mass ratio of 1:(20-30), the pH was adjusted to 4-6 with 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 10-30°C and 200-300 r / min for 20-30 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol were mixed at a mass ratio of 1:(50-60), 8-10 times the mass of the nano-attapulgite was added with the silane hydrolyzate, and the mixture was stirred at 50-60°C and 300-500 r / min for 1-2 h, filtered, and dried at 5-7 Pa and 50-60°C for 6-7 h to prepare a pretreated nano-attapulgite; the pretreated nano-attapulgite, modified DOPO, and N,N-dimethylformamide were mixed at a mass ratio of 1:(50-60). :(2~3):(20~30) are mixed evenly, and stirred at 50~60℃, 300~500r / min for 2~3h under nitrogen atmosphere, filtered, washed with anhydrous ethanol for 3~5 times, and dried at 5~7Pa, 50~60℃ for 6~7h to obtain pre-modified nano-attapulgite; pre-modified nano-attapulgite, 3-maleimidopropionic acid, sodium hydroxide, N,N-dimethylformamide are mixed evenly in a mass ratio of 1:(2~3):(0.04~0.06):(20~24), stirred at 90~100℃, 300~500r / min for 3~4h, filtered, washed with anhydrous ethanol and deionized water for 3~5 times respectively, and dried at 5~7Pa, 50~60℃ for 6~7h to obtain modified nano-attapulgite;
[0013] (5) The acrylic copolymer emulsion, modified nano-attapulgite and defoamer were mixed evenly in a mass ratio of 1: (0.05-0.07): (0.02-0.04), stirred at 10-30 ° C and 300-500 r / min for 20-30 min, and the viscosity was adjusted to 60-80 KU with deionized water to prepare a self-healing flame retardant coating.
[0014] As an optimization, the reaction process of the acrylic copolymer emulsion in step (2) is:
[0015] .
[0016] As an optimization, the reaction process of the modified DOPO in step (3) is:
[0017] .
[0018] As an optimization, the reaction process of the modified nano-attapulgite in step (4) is:
[0019] .
[0020] As an optimization, the model of the polyether nonionic emulsifier in step (2) is AE-100.
[0021] As an optimization, the defoaming agent in step (5) is of model THIX-318.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] When preparing the self-repairing flame-retardant coating, the present invention comprises the following steps: reacting allyl glycidyl ether with 9-anthracene carboxylic acid to obtain allyl anthracene monomer; reacting methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate and allyl anthracene monomer to obtain acrylate copolymer emulsion; reacting diethanolamine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide to obtain modified DOPO; reacting nano-attapulgite with 3-isocyanatopropyltriethoxysilane, modified DOPO and 3-maleimide propionic acid in sequence to obtain modified nano-attapulgite; and uniformly mixing the acrylate copolymer emulsion, the modified nano-attapulgite and a defoamer to obtain the self-repairing flame-retardant coating.
[0024] Firstly, allyl glycidyl ether is reacted with 9-anthracenecarboxylic acid to obtain allyl anthracene monomer. Allyl anthracene monomer can participate in the copolymerization reaction of acrylate copolymer. Anthracene group is introduced into the side chain of acrylate copolymer molecule. The anthracene group can react with the maleimide group on the modified nano-attapulgite to form a thermally reversible cross-linking network, which gives the self-healing flame-retardant coating excellent self-healing properties. Methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate and allyl anthracene monomers are reacted to obtain acrylate copolymer emulsion, and fluorine atoms are introduced into the side chain of acrylate copolymer molecule. Fluorine atoms have low reactivity and hydrophobicity, which can give the self-healing flame-retardant coating excellent corrosion resistance.
[0025] Secondly, diethanolamine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide are reacted to obtain modified DOPO; nano-attapulgite is reacted with 3-isocyanatopropyltriethoxysilane to obtain pretreated nano-attapulgite, and isocyanate is introduced into the pretreated nano-attapulgite; the pretreated nano-attapulgite is reacted with modified DOPO to obtain pre-modified nano-attapulgite, the isocyanate on the pretreated nano-attapulgite reacts with the hydroxyl group at one end of the modified DOPO, and the DOPO structure and hydroxyl group are introduced into the pre-modified nano-attapulgite, and the introduction of the DOPO structure can give the self-healing flame-retardant coating excellent flame retardant properties; the pre-modified nano-attapulgite is reacted with 3-maleimide propionic acid to obtain modified nano-attapulgite. Attapulgite; the hydroxyl group on the pre-modified nano-attapulgite is esterified with the carboxyl group on 3-maleimidopropionic acid, and a maleimide group is introduced into the modified nano-attapulgite. The maleimide group on the modified nano-attapulgite can undergo a Diels-Alder addition reaction with the anthracene group introduced on the side chain of the acrylate copolymer molecule to form a thermally reversible cross-linked network, thereby giving the self-healing flame-retardant coating excellent self-healing properties; Nano-attapulgite is a two-dimensional inorganic nanomaterial that can form a physical barrier in the self-healing flame-retardant coating, causing a tortuous effect in the diffusion process of the penetrating molecules, extending the diffusion path, and improving the barrier properties of the self-healing flame-retardant coating, isolating the penetration of gases and liquids, and giving the self-healing flame-retardant coating excellent corrosion resistance. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Example 1
[0028] A method for preparing a self-repairing flame retardant coating, the method for preparing the self-repairing flame retardant coating comprising the following preparation steps:
[0029] (1) Allyl glycidyl ether and 9-anthracenecarboxylic acid were added in a molar ratio of 1:1 to tetrahydrofuran (18 times the mass of allyl glycidyl ether), stirred at 60°C and 300 r / min for 24 hours, and dried at 5Pa and 50°C for 7 hours to obtain an allyl anthracene monomer;
[0030] (2) Methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate and allyl anthracene monomers were mixed at a mass ratio of 1:1:0.1:0.1 to prepare a mixed monomer; 0.01 times the mass of the mixed monomer and potassium persulfate and deionized water were mixed at a mass ratio of 1:20 to prepare a potassium persulfate aqueous solution; 0.05 times the mass of the mixed monomer and polyether nonionic emulsifier were mixed at a mass ratio of 1:180, the temperature was raised to 70°C, and 8% of the total amount of the mixed monomer and 8% of the total amount of the potassium persulfate aqueous solution were uniformly added dropwise within 10 minutes, and the mixture was stirred at 70°C and 300 r / min for 17 minutes to prepare a seed emulsion; the remaining mixed monomer and potassium persulfate aqueous solution were uniformly added dropwise to the seed emulsion within 2 hours, and the mixture was stirred at 80°C and 300 r / min for 50 minutes, and the mixture was cooled to room temperature and filtered to prepare an acrylate copolymer emulsion;
[0031] (3) Add diethanolamine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and triethylamine in a molar ratio of 1:1:1 to dichloromethane (8 times the mass of diethanolamine), cool to -10°C, and under nitrogen atmosphere, add carbon tetrachloride (0.04 times the mass of diethanolamine) dropwise at a constant rate of 300 r / min under stirring conditions within 10 minutes. Continue stirring and reacting for 24 hours, filter, and wash the filtrate with 8% sodium bicarbonate aqueous solution and saturated sodium chloride aqueous solution three times each, and dry at 5 Pa and 40°C for 7 hours to obtain modified DOPO;
[0032] (4) 3-isocyanatopropyltriethoxysilane and deionized water were mixed at a mass ratio of 1:20, the pH was adjusted to 4 with 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 10°C and 200 r / min for 30 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol were mixed at a mass ratio of 1:50, silane hydrolyzate with a mass of 8 times that of the nano-attapulgite was added, and the mixture was stirred at 50°C and 300 r / min for 2 h, filtered, and dried at 5 Pa and 50°C for 7 h to prepare pretreated nano-attapulgite; the pretreated nano-attapulgite, modified DOPO, and N,N-dimethyl The pre-modified nano-attapulgite was prepared by mixing the pre-modified nano-attapulgite, 3-maleimidopropionic acid, sodium hydroxide and N,N-dimethylformamide in a mass ratio of 1:2:0.04:20, stirring and reacting at 90°C and 300r / min for 4h, filtering, washing with anhydrous ethanol and deionized water for 3 times respectively, and drying at 5Pa and 50°C for 7h to obtain the modified nano-attapulgite.
[0033] (5) The acrylic copolymer emulsion, modified nano-attapulgite and defoamer were mixed evenly in a mass ratio of 1:0.05:0.02, stirred at 10°C and 300 r / min for 30 min, and the viscosity was adjusted to 60 KU with deionized water to prepare a self-healing flame retardant coating.
[0034] Example 2
[0035] A method for preparing a self-repairing flame retardant coating, the method for preparing the self-repairing flame retardant coating comprising the following preparation steps:
[0036] (1) Allyl glycidyl ether and 9-anthracenecarboxylic acid were added to tetrahydrofuran (19 times the mass of allyl glycidyl ether) in a molar ratio of 1:1, stirred at 62°C and 400 r / min for 22 hours, and dried at 6Pa and 55°C for 6.5 hours to obtain allyl anthracene monomer;
[0037] (2) Methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate and allyl anthracene monomers were mixed at a mass ratio of 1:1:0.15:0.15 to prepare a mixed monomer; 0.02 times the mass of the mixed monomer and deionized water were mixed at a mass ratio of 1:25 to prepare a potassium persulfate aqueous solution; 0.06 times the mass of the mixed monomer and a polyether nonionic emulsifier were mixed at a mass ratio of 1:190 to prepare a mixed monomer solution, the mixture was heated to 75°C, 9% of the total amount of the mixed monomer and 9% of the total amount of the potassium persulfate aqueous solution were added dropwise at a constant speed within 10 minutes, the mixture was stirred at 75°C and 400 r / min for 16 minutes to prepare a seed emulsion; the remaining mixed monomer and potassium persulfate aqueous solution were added dropwise to the seed emulsion at a constant speed within 2.5 hours, the mixture was stirred at 85°C and 400 r / min for 45 minutes, the mixture was cooled to room temperature, and the mixture was filtered to prepare an acrylate copolymer emulsion;
[0038] (3) Add diethanolamine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and triethylamine in a molar ratio of 1:1:1 to dichloromethane (9 times the mass of diethanolamine), cool to -5°C, and add carbon tetrachloride (0.05 times the mass of diethanolamine) dropwise at a constant rate of 10 min under a nitrogen atmosphere and stirring at 400 r / min. Continue stirring and reacting for 22 h, filter, and wash the filtrate with a 9% sodium bicarbonate aqueous solution and a saturated sodium chloride aqueous solution 4 times each, and dry at 6 Pa and 45°C for 6.5 h to obtain modified DOPO;
[0039] (4) 3-isocyanatopropyltriethoxysilane and deionized water were mixed at a mass ratio of 1:25, the pH was adjusted to 5 with 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 20°C and 250 r / min for 25 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol were mixed at a mass ratio of 1:55, 9 times the mass of the nano-attapulgite was added with the silane hydrolyzate, and the mixture was stirred at 55°C and 400 r / min for 1.5 h, filtered, and dried at 6 Pa and 55°C for 6.5 h to prepare a pretreated nano-attapulgite; the pretreated nano-attapulgite, modified DOPO, and N,N-dimethylformamide were mixed. The pre-modified nano-attapulgite was prepared by mixing the pre-modified nano-attapulgite, 3-maleimidopropionic acid, sodium hydroxide and N,N-dimethylformamide in a mass ratio of 1:2.5:0.05:22, stirring at 95°C and 400r / min for 3.5h, filtering, washing with anhydrous ethanol and deionized water for 4 times, and drying at 6Pa and 55°C for 6.5h to obtain the modified nano-attapulgite.
[0040] (5) The acrylic copolymer emulsion, modified nano-attapulgite and defoamer were mixed evenly in a mass ratio of 1:0.06:0.03, stirred at 20°C and 400 r / min for 25 min, and the viscosity was adjusted to 70 KU with deionized water to prepare a self-healing flame retardant coating.
[0041] Example 3
[0042] A method for preparing a self-repairing flame retardant coating, the method for preparing the self-repairing flame retardant coating comprising the following preparation steps:
[0043] (1) Allyl glycidyl ether and 9-anthracenecarboxylic acid were added to tetrahydrofuran (20 times the mass of allyl glycidyl ether) in a molar ratio of 1:1, stirred at 64°C and 500 r / min for 20 h, and dried at 7 Pa and 60°C for 6 h to obtain allyl anthracene monomer;
[0044] (2) Methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate and allyl anthracene monomers were mixed at a mass ratio of 1:1:0.2:0.2 to prepare a mixed monomer; 0.03 times the mass of the mixed monomer and deionized water were mixed at a mass ratio of 1:30 to prepare a potassium persulfate aqueous solution; 0.07 times the mass of the mixed monomer and a polyether nonionic emulsifier were mixed at a mass ratio of 1:200 to prepare a potassium persulfate aqueous solution, the mixture was heated to 80°C, 10% of the total amount of the mixed monomer and 10% of the total amount of the potassium persulfate aqueous solution were uniformly added dropwise within 10 minutes, and the mixture was stirred at 80°C and 500 r / min for 15 minutes to prepare a seed emulsion; the remaining mixed monomer and potassium persulfate aqueous solution were uniformly added dropwise to the seed emulsion within 3 hours, and the mixture was stirred at 90°C and 500 r / min for 40 minutes, cooled to room temperature, filtered, and an acrylate copolymer emulsion was prepared;
[0045] (3) Add diethanolamine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and triethylamine in a molar ratio of 1:1:1 to dichloromethane (10 times the mass of diethanolamine), cool to 0°C, and add carbon tetrachloride (0.06 times the mass of diethanolamine) dropwise at a constant rate of 500 r / min under a nitrogen atmosphere for 10 minutes. Continue stirring and reacting for 20 hours, filter, and wash the filtrate with a 10% sodium bicarbonate aqueous solution and a saturated sodium chloride aqueous solution for 5 times each, and dry at 7 Pa and 50°C for 6 hours to obtain modified DOPO;
[0046] (4) 3-isocyanatopropyltriethoxysilane and deionized water were mixed at a mass ratio of 1:30, the pH was adjusted to 6 with 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 30°C and 300 r / min for 20 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol were mixed at a mass ratio of 1:60, and 10 times the mass of the nano-attapulgite was added with silane hydrolyzate, and the mixture was stirred at 60°C and 500 r / min for 1 h, filtered, and dried at 7 Pa and 60°C for 6 h to prepare pretreated nano-attapulgite; the pretreated nano-attapulgite, modified DOPO, and N,N-dimethyl The pre-modified nano-attapulgite was prepared by mixing the pre-modified nano-attapulgite, 3-maleimidopropionic acid, sodium hydroxide and N,N-dimethylformamide in a mass ratio of 1:3:0.06:24, stirring and reacting at 100°C and 500r / min for 3h, filtering, washing with anhydrous ethanol and deionized water for 5 times respectively, and drying at 7Pa and 60°C for 6h to obtain the modified nano-attapulgite.
[0047] (5) The acrylic copolymer emulsion, modified nano-attapulgite and defoamer were mixed evenly in a mass ratio of 1:0.07:0.04, stirred at 30°C and 500 r / min for 20 min, and the viscosity was adjusted to 80 KU with deionized water to prepare a self-healing flame retardant coating.
[0048] Comparative Example 1
[0049] The preparation method of the self-healing flame retardant coating of Comparative Example 1 is different from that of Example 2 in that step (1) is not performed, and step (2) is modified as follows: methyl acrylate, ethyl acrylate, and 2-(perfluorohexyl)ethyl methacrylate are mixed uniformly in a mass ratio of 1:1:0.15 to prepare a mixed monomer; 0.02 times the mass of the mixed monomer and potassium persulfate and deionized water are mixed uniformly in a mass ratio of 1:25 to prepare a potassium persulfate aqueous solution; 0.06 times the mass of the mixed monomer and a polyether nonionic emulsifier are mixed with deionized water. The mixture was uniformly mixed with water at a mass ratio of 1:190, heated to 75°C, and a mixed monomer of 9% of the total amount of the mixed monomer and a potassium persulfate aqueous solution of 9% of the total amount of the potassium persulfate aqueous solution were uniformly added dropwise within 10 minutes, and stirred at 75°C and 400 r / min for 16 minutes to obtain a seed emulsion; the remaining mixed monomer and potassium persulfate aqueous solution were uniformly added dropwise to the seed emulsion within 2.5 hours, stirred at 85°C and 400 r / min for 45 minutes, cooled to room temperature, filtered, and an acrylate copolymer emulsion was obtained. The remaining steps are the same as in Example 2.
[0050] Comparative Example 2
[0051] The preparation method of the self-healing flame retardant coating of Comparative Example 2 is different from that of Example 2 in that step (2) is different. Step (2) is modified as follows: methyl acrylate, ethyl acrylate, and allyl anthracene monomers are mixed uniformly in a mass ratio of 1:1:0.15 to prepare a mixed monomer; potassium persulfate (0.02 times the mass of the mixed monomer) and deionized water are mixed uniformly in a mass ratio of 1:25 to prepare a potassium persulfate aqueous solution; a polyether nonionic emulsifier (0.06 times the mass of the mixed monomer) and deionized water are mixed uniformly in a mass ratio of 1:190, mix evenly, heat to 75°C, uniformly add 9% of the total amount of the mixed monomers and 9% of the total amount of the potassium persulfate aqueous solution within 10 minutes, stir at 75°C, 400r / min for 16 minutes to obtain a seed emulsion; uniformly add the remaining mixed monomers and potassium persulfate aqueous solution to the seed emulsion within 2.5 hours, stir at 85°C, 400r / min for 45 minutes, cool to room temperature, filter, and obtain an acrylate copolymer emulsion. The remaining steps are the same as in Example 2.
[0052] Comparative Example 3
[0053] The preparation method of the self-healing flame-retardant coating of Comparative Example 3 is different from that of Example 2 in that step (3) is not performed, and step (4) is modified as follows: 3-mercaptopropyltriethoxysilane and deionized water are mixed uniformly in a mass ratio of 1:25, the pH value is adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and the mixture is stirred at 20°C and 250 r / min for 25 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol are mixed uniformly in a mass ratio of 1:55, and a silane hydrolyzate of 9 times the mass of the nano-attapulgite is added, and the mixture is stirred at 20°C and 250 r / min for 25 min to prepare a silane hydrolyzate. 55°C, 400r / min stirring reaction for 1.5h, filtered, 6Pa, 55°C drying for 6.5h, to obtain pretreated nano-attapulgite; pretreated nano-attapulgite, N-allylmaleimide, azobisisobutyronitrile, N,N-dimethylformamide were mixed uniformly in a mass ratio of 1:2.5:0.02:25, stirred at 55°C, 400r / min for 2.5h, filtered, washed with anhydrous ethanol 4 times, and dried at 6Pa, 55°C for 6.5h to obtain modified nano-attapulgite. The remaining steps are the same as in Example 2.
[0054] Comparative Example 4
[0055] The preparation method of the self-healing flame-retardant coating of Comparative Example 4 is different from that of Example 2 only in step (4). Step (4) is modified as follows: 3-isocyanatepropyltriethoxysilane and deionized water are mixed at a mass ratio of 1:25, the pH value is adjusted to 5 with a 1 mol / L oxalic acid aqueous solution, and stirred at 20°C and 250 r / min for 25 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol are mixed at a mass ratio of 1:55, and 9 times the mass of nano-attapulgite is added. The silane hydrolyzate was stirred at 55°C and 400r / min for 1.5h, filtered, and dried at 6Pa and 55°C for 6.5h to obtain pretreated nano-attapulgite; the pretreated nano-attapulgite, modified DOPO, and N,N-dimethylformamide were mixed uniformly at a mass ratio of 1:2.5:25, stirred at 55°C and 400r / min for 2.5h under a nitrogen atmosphere, filtered, washed with anhydrous ethanol 4 times, and dried at 6Pa and 55°C for 6.5h to obtain modified nano-attapulgite. The remaining steps were the same as in Example 2.
[0056] Comparative Example 5
[0057] The preparation method of the self-repairing flame-retardant coating of Comparative Example 5 is different from that of Example 2 in that step (3) and step (4) are not performed, and step (5) is modified as follows: the acrylic copolymer emulsion and the defoamer are mixed uniformly at a mass ratio of 1:0.03, stirred at 20°C and 400 r / min for 25 min, and the viscosity is adjusted to 70 KU with deionized water to prepare the self-repairing flame-retardant coating. The remaining steps are the same as those of Example 2.
[0058] Test Example 1
[0059] Flame retardant performance test
[0060] Test method: Pour the examples and comparative examples into a polytetrafluoroethylene mold and cure them at room temperature for 24 hours. Cut the cured samples into standard strips according to GB / T2406.2 and test the limiting oxygen index of the standard strips.
[0061] The results are shown in Table 1
[0062] .
[0063] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 1, it can be found that the self-repairing flame-retardant coating prepared by the present invention has good flame-retardant properties.
[0064] By comparison, the limiting oxygen index of Examples 1 to 3 is greater than that of Comparative Example 3 and Comparative Example 5, indicating that diethanolamine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide are reacted to obtain modified DOPO; nano-attapulgite is reacted with 3-isocyanatepropyltriethoxysilane to obtain pretreated nano-attapulgite, and isocyanate is introduced into the pretreated nano-attapulgite; the pretreated nano-attapulgite is reacted with modified DOPO to obtain pre-modified nano-attapulgite, the isocyanate on the pretreated nano-attapulgite reacts with the hydroxyl group at one end of the modified DOPO, and the DOPO structure is introduced into the pre-modified nano-attapulgite, and the introduction of the DOPO structure can give the self-healing flame-retardant coating excellent flame retardant properties.
[0065] Test Example 2
[0066] Self-healing performance test
[0067] Test method: Pour the embodiment and comparative example into a polytetrafluoroethylene mold, cure at room temperature for 24 hours, cut the cured sample into standard specimens according to GB / T1040.1, and test its original tensile strength with a tensile machine. Then, cut a 2mm deep and 10mm long crack in the middle of the unstretched original specimen, place it in the mold, keep it at 70°C for 4 hours, and let it stand at room temperature for 10 hours to obtain the repaired specimen. Test its tensile strength with a tensile machine. Calculate the self-repair rate of the embodiment and comparative example before and after repair, self-repair rate = (tensile strength of the specimen after repair / original tensile strength of the specimen) × 100%.
[0068] The results are shown in Table 2
[0069] .
[0070] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 2, it can be found that the self-repairing flame retardant coating prepared by the present invention has good self-repairing performance.
[0071] By comparison, the self-repairing rates of Examples 1 to 3 are greater than that of Comparative Example 1, indicating that allyl glycidyl ether is reacted with 9-anthracenecarboxylic acid to obtain allyl anthracene monomers, and allyl anthracene monomers can participate in the copolymerization reaction of the acrylate copolymer, and anthracene groups are introduced into the side chains of the acrylate copolymer molecules. The anthracene groups can undergo Diels-Alder addition reactions with the maleimide groups on the modified nano-attapulgite to form a thermally reversible cross-linked network, thereby giving the self-repairing flame-retardant coating excellent self-repairing properties.
[0072] By comparison, the self-healing rates of Examples 1 to 3 are greater than those of Comparative Examples 4 to 5, indicating that the modified nano-attapulgite is prepared by reacting the pre-modified nano-attapulgite with 3-maleimidopropionic acid; the hydroxyl group on the pre-modified nano-attapulgite is esterified with the carboxyl group on the 3-maleimidopropionic acid, and a maleimide group is introduced into the modified nano-attapulgite. The maleimide group on the modified nano-attapulgite can undergo a Diels-Alder addition reaction with the anthracene group introduced on the side chain of the acrylate copolymer molecule to form a thermally reversible cross-linked network, thereby giving the self-healing flame-retardant coating excellent self-healing properties.
[0073] Test Example 3
[0074] Corrosion resistance test
[0075] Test method: The examples and comparative examples were evenly coated on a steel sample with a size of 10 mm × 10 mm × 100 mm, cured at room temperature for 24 hours and weighed, recorded as m 1 The weighed steel specimen was immersed in a 10% hydrochloric acid aqueous solution, left to stand for 24 hours, taken out, placed in an oven, dried at 7Pa, 60℃ for 10 hours, and weighed, recorded as m 2 , calculate the corrosion rate of the embodiment and the comparative example, corrosion rate = (m 1 -m 2 ) / m 1 ×%.
[0076] The results are shown in Table 3
[0077] .
[0078] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 5 in Table 3, it can be found that the self-repairing flame retardant coating prepared by the present invention has good corrosion resistance.
[0079] By comparison, the corrosion rates of Examples 1 to 3 are lower than that of Comparative Example 2, indicating that methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate, and allyl anthracene monomers are reacted to prepare an acrylate copolymer emulsion, and fluorine atoms are introduced into the side chains of the acrylate copolymer molecules. Fluorine atoms have low reactivity and hydrophobicity, and can give the self-healing flame retardant coating excellent corrosion resistance.
[0080] By comparison, the corrosion rates of Examples 1 to 3 are lower than that of Comparative Example 5, indicating that the self-healing flame retardant coating is prepared by uniformly mixing the acrylate copolymer emulsion, modified nano-attapulgite and defoaming agent; nano-attapulgite is a two-dimensional inorganic nanomaterial, which can form a physical barrier in the self-healing flame retardant coating, causing the diffusion process of the penetrating molecules to produce a tortuous effect, extending the diffusion path, and improving the barrier properties of the self-healing flame retardant coating, giving the self-healing flame retardant coating excellent corrosion resistance.
[0081] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A self-repairing flame retardant coating, It is characterized in that The self-repairing flame-retardant coating is prepared by reacting methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate, and allyl anthracene monomers to obtain an acrylate copolymer emulsion; reacting nano-attapulgite with 3-isocyanatopropyltriethoxysilane, modified DOPO, and 3-maleimide propionic acid in sequence to obtain modified nano-attapulgite; and uniformly mixing the acrylate copolymer emulsion, the modified nano-attapulgite, and a defoamer. The allyl anthracene monomer is prepared by reacting allyl glycidyl ether with 9-anthracenecarboxylic acid; The modified DOPO is prepared by reacting diethanolamine and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
2. A method for preparing a self-repairing flame retardant coating, It is characterized in that The method comprises the following preparation steps: (1) adding allyl glycidyl ether and 9-anthracenecarboxylic acid in a molar ratio of 1:1 to tetrahydrofuran (18 to 20 times the mass of allyl glycidyl ether), stirring at 60 to 64°C and 300 to 500 r / min for 20 to 24 hours, and drying at 5 to 7 Pa and 50 to 60°C for 6 to 7 hours to obtain allyl anthracene monomer; (2) Methyl acrylate, ethyl acrylate, 2-(perfluorohexyl)ethyl methacrylate, and allyl anthracene monomers are mixed at a mass ratio of 1:1:(0.1~0.2):(0.1~0.2) to prepare a mixed monomer; potassium persulfate (0.01~0.03 times the mass of the mixed monomer) and deionized water are mixed at a mass ratio of 1:(20~30) to prepare a potassium persulfate aqueous solution; polyether nonionic emulsifier (0.05~0.07 times the mass of the mixed monomer) and deionized water are mixed at a mass ratio of 1:(180~200) to prepare a mixed monomer solution; , raise the temperature to 70-80°C, uniformly add 8-10% of the total amount of the mixed monomers and 8-10% of the total amount of the potassium persulfate aqueous solution within 10 minutes, stir and react at 70-80°C, 300-500r / min for 15-17 minutes to obtain a seed emulsion; uniformly add the remaining mixed monomers and the potassium persulfate aqueous solution to the seed emulsion within 2-3 hours, stir and react at 80-90°C, 300-500r / min for 40-50 minutes, cool to room temperature, filter, and obtain an acrylate copolymer emulsion; (3) Add diethanolamine, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and triethylamine in a molar ratio of 1:1:1 to dichloromethane (8 to 10 times the mass of diethanolamine), cool to -10 to 0°C, and under a nitrogen atmosphere, add carbon tetrachloride (0.04 to 0.06 times the mass of diethanolamine) dropwise at a constant rate within 10 minutes at a stirring rate of 300 to 500 r / min. Continue stirring and reacting for 20 to 24 hours, filter, and wash the filtrate with a sodium bicarbonate aqueous solution (8 to 10% by mass) and a saturated sodium chloride aqueous solution (3 to 5 times each), and dry at 5 to 7 Pa and 40 to 50°C for 6 to 7 hours to obtain modified DOPO; (4) 3-isocyanatopropyltriethoxysilane and deionized water were mixed at a mass ratio of 1:(20-30), the pH was adjusted to 4-6 with 1 mol / L oxalic acid aqueous solution, and the mixture was stirred at 10-30°C and 200-300 r / min for 20-30 min to prepare a silane hydrolyzate; nano-attapulgite and anhydrous ethanol were mixed at a mass ratio of 1:(50-60), 8-10 times the mass of the nano-attapulgite was added with the silane hydrolyzate, and the mixture was stirred at 50-60°C and 300-500 r / min for 1-2 h, filtered, and dried at 5-7 Pa and 50-60°C for 6-7 h to obtain pretreated nano-attapulgite; The pretreated nano-attapulgite, modified DOPO and N,N-dimethylformamide were uniformly mixed in a mass ratio of 1:(2-3):(20-30), stirred at 50-60°C and 300-500r / min for 2-3h under a nitrogen atmosphere, filtered, washed with anhydrous ethanol for 3-5 times, and dried at 50-60°C and 5-7Pa for 6-7h to obtain pre-modified nano-attapulgite; the pre-modified nano-attapulgite was , 3-maleimidopropionic acid, sodium hydroxide, N,N-dimethylformamide are mixed uniformly in a mass ratio of 1:(2-3):(0.04-0.06):(20-24), stirred at 90-100°C, 300-500r / min for 3-4h, filtered, washed with anhydrous ethanol and deionized water for 3-5 times respectively, dried at 5-7Pa, 50-60°C for 6-7h to obtain modified nano-attapulgite; (5) The acrylic copolymer emulsion, modified nano-attapulgite and defoamer were mixed evenly in a mass ratio of 1: (0.05-0.07): (0.02-0.04), stirred at 10-30 ° C and 300-500 r / min for 20-30 min, and the viscosity was adjusted to 60-80 KU with deionized water to prepare a self-healing flame retardant coating.
3. A method for preparing a self-repairing flame-retardant coating according to claim 2, It is characterized in that The reaction process of the acrylic copolymer emulsion in step (2) is: 。 4. A method for preparing a self-repairing flame retardant coating according to claim 2, It is characterized in that The reaction process of the modified DOPO in step (3) is: 。 5. A method for preparing a self-repairing flame retardant coating according to claim 2, It is characterized in that The reaction process of the modified nano-attapulgite in step (4) is: 。 6. A method for preparing a self-repairing flame retardant coating according to claim 2, It is characterized in that The model of the polyether nonionic emulsifier in step (2) is AE-100.
7. A method for preparing a self-repairing flame-retardant coating according to claim 2, It is characterized in that The model of the defoaming agent in step (5) is THIX-318.