A kind of SBS modified asphalt and preparation method thereof
By using modified nanomaterials and hindered phenol structures in SBS modified asphalt, a dense network structure is formed, which solves the problem of insufficient anti-aging and mechanical properties of asphalt in the existing technology, and achieves efficient anti-aging and storage stability of asphalt. promote.
Patent Information
- Application Number
- CN202410366409.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing SBS modified asphalt still has deficiencies in aging resistance, mechanical properties and storage stability, making it difficult to meet actual application needs.
Using SBS and modified nanomaterials to synergize, by preparing HNTs@MPS nanomaterials and modified titanium dioxide, combined with hindered phenol structure and mesoporous silica, a dense network structure is formed to improve the mechanical properties and anti-aging properties of asphalt, and The storage stability of asphalt is enhanced through the covering of nano-titanium dioxide and the absorption of mesoporous silica.
It significantly improves the anti-aging properties, mechanical properties and storage stability of asphalt, enhances the high-temperature shear deformation resistance of asphalt, reduces rutting and environmental pollution, and extends the service life of asphalt.
Smart Images

Figure BDA0004764364430000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of asphalt materials, and in particular to an SBS modified asphalt and a preparation method thereof. Background Art
[0002] The surface of asphalt is black and mostly exists in liquid or semi-solid state. It is composed of hydrocarbons of different molecular weights and their non-metallic derivatives. It has high viscosity and is widely used in industrial fields such as coatings, plastics, rubber, and road paving. SBS is a styrene block copolymer with a multiphase structure. The polystyrene block (S segment) connects the two ends of the polybutadiene block (B segment) to play a restraining role. When SBS is mixed with the matrix asphalt, it will interact with the asphalt components to swell. When the SBS content is high, the SBS molecules will form a stable network structure in the asphalt, thereby improving the road performance of the modified asphalt. However, using SBS alone to modify asphalt no longer meets the actual application needs.
[0003] Some researchers have found that using nanomaterials and SBS as a composite modification system to modify asphalt can not only improve the poor compatibility of polymer-modified asphalt, and the susceptibility to UV aging and oxidative aging, but also improve the mechanical properties of asphalt. Therefore, it is necessary to develop an SBS-modified asphalt with excellent anti-aging properties, mechanical properties and storage stability. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an SBS modified asphalt and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An SBS modified asphalt comprises the following raw materials in parts by weight: 100 parts of asphalt, 3-7 parts of SBS, 2-10 parts of modified nanomaterials, and 0.2-0.8 parts of stabilizer;
[0007] The modified nanomaterial is prepared by the following steps:
[0008] Step A1, mixing halloysite nanotubes, hexadecyltrimethylammonium bromide and deionized water in a reactor, and then ultrasonically treating for 30-60 minutes, adjusting the pH of the system to 8-12, and then adding tetraethyl orthosilicate and KH550 dropwise, and maintaining the system temperature at 30-50° C., stirring and reacting for 4-8 hours, after the reaction is completed, washing and filtering, dispersing the filter cake in acetone and ultrasonicating for 30 minutes, placing it at 80-100° C. and refluxing for 8-10 hours, washing, filtering, adding an equal amount of acetone and continuing to reflux for 8-10 hours, washing, filtering, and vacuum drying at 60° C. for 8-12 hours to obtain HNTs@MPS nanomaterials;
[0009] Further, the usage ratio of halloysite nanotubes, hexadecyltrimethylammonium bromide, deionized water, tetraethyl orthosilicate, KH550 and acetone is 1 g: 2-4 g: 200 mL: 3-4 mL: 2.21-3.32-4.42 g: 400 mL.
[0010] Step A2, stirring and mixing nano titanium dioxide, KH550, ethanol and deionized water in a reactor, raising the system temperature to 40-80°C, continuing to stir and react for 3-5 hours, centrifuging and washing after the reaction is completed, re-dispersing the precipitate in acetone and ultrasonicating for 30 minutes, and controlling the system temperature at 0-5°C, adding cyanuric chloride and triethylamine, stirring and reacting for 3-5 hours, and centrifuging, washing and drying after the reaction is completed to obtain modified titanium dioxide;
[0011] Furthermore, the usage ratio of nano titanium dioxide, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 1-2g: 2.21-3.32-4.42g: 50mL: 10mL: 100mL: 1.84-2.76-3.68g: 1-3g.
[0012] Step A3, 4-amino-2,6-di-tert-butylphenol and acetone are mixed evenly in a beaker, recorded as solution 1, HNTs@MPS nanomaterials and acetone are mixed evenly in a beaker, recorded as solution 2, modified titanium dioxide and acetone are added to a reactor and mixed evenly, then solution 1 is slowly added dropwise to the above solution, and the system temperature is controlled to be 40-50° C., and then half of the 0.1 mol / L sodium hydroxide solution is slowly added dropwise, and the reaction is carried out for 3-4 hours, and the system temperature is continuously raised to 85-95° C., and then solution 2 and the remaining sodium hydroxide solution are slowly added dropwise, and the reaction is continued for 5-7 hours. After the reaction is completed, centrifugation, washing, and drying are performed to obtain the modified nanomaterial;
[0013] Furthermore, the dosage ratio of modified titanium dioxide, acetone, solution 1, solution 2 and sodium hydroxide solution is 1-2 g: 200 mL: 20 mL: 20 mL: 40-80 mL; the dosage ratio of 4-amino-2,6-di-tert-butylphenol and acetone in solution 1 is 2.21-4.42 g: 20 mL, and the dosage ratio of HNTs@MPS nanomaterials and acetone in solution 2 is 1.5-2.5 g: 20 mL.
[0014] A method for preparing SBS modified asphalt comprises the following steps:
[0015] Weigh the raw materials according to the weight fraction, heat the asphalt to 160-180°C, stir, then add SBS, modified nanomaterials and stabilizer, stir and shear for 2.5-4.5 hours to obtain SBS modified asphalt.
[0016] Beneficial effects of the present invention:
[0017] During the preparation process of the SBS modified asphalt of the present invention, the synergistic effect between SBS and modified nanomaterials is utilized to improve the storage stability of the asphalt, and the halloysite nanotubes are used as a toughening substrate to improve the mechanical properties of the asphalt matrix. The asphalt is modified to introduce a hindered phenol structure, nano-titanium dioxide and mesoporous silica to improve the anti-aging performance of the matrix.
[0018] In the modified nanomaterials, first, halloysite nanotubes are used as toughening substrates, and a layer of mesoporous silica is coated on their surface using tetraethyl orthosilicate and KH550 as silicon sources and hexadecyltrimethylammonium bromide as a template to synthesize HNTs@MPS nanomaterials containing amino groups on the surface; secondly, KH550 is used to introduce amino groups on the surface of titanium dioxide, and then cyanuric chloride is used to react with amino groups to synthesize modified titanium dioxide, thereby introducing triazine groups; finally, cyanuric chloride on the surface of modified titanium dioxide is used as an intermediate to connect the HNTs@MPS nanomaterials containing amino groups and hindered phenol structures to synthesize modified nanomaterials. After the modified nanomaterials are added to the matrix, the halloysite nanotubes, due to their large aspect ratio and high temperature resistance, can play an interactive connection role between SBS and the matrix asphalt, forming a denser "network" structure. When subjected to load, the halloysite nanotubes play a reinforcing role in the asphalt, slowing down the tensile damage of the interface between SBS and asphalt, and improving the high-temperature shear deformation resistance of asphalt, which makes the modified asphalt have good elastic recovery ability and can reduce rutting; the mesoporous silica coated on the surface of the halloysite nanotubes can enhance the strength and hardness of the modified asphalt matrix, reduce the occurrence of problems such as cracking and warping at the asphalt interface, and when used as a road paving material, the uniform pore structure of mesoporous silica can also be used to absorb exhaust gas generated by automobiles to reduce environmental pollution; in addition, hindered phenol structure and nano titanium dioxide The mesoporous silica is connected with asphalt by cyanuric chloride, which avoids the loss caused by migration, volatilization and thermal decomposition, and works synergistically. The three work synergistically to greatly improve the anti-aging performance of asphalt. Among them, the hindered structure can eliminate the free radicals in the asphalt, thereby avoiding the free radical chain reaction of organic matter in the asphalt. Nano-titanium dioxide has excellent covering power and refractive power, has a good shielding effect on ultraviolet light, and has an auxiliary antioxidant effect. Mesoporous silica absorbs part of the light energy and reflects thermal radiation, thereby reducing the temperature of the asphalt interface and indirectly slowing down the aging rate. The modified nanomaterial also has a large specific surface area, can be well integrated with asphalt, effectively restricts the movement of SBS molecular chains, improves the interaction between SBS and asphalt, and improves the storage stability of asphalt. DETAILED DESCRIPTION
[0019] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Example 1
[0021] The modified nanomaterials are prepared by the following steps:
[0022] Step A1, halloysite nanotubes, hexadecyltrimethylammonium bromide and deionized water are mixed in a reactor, and then ultrasonically treated for 30 minutes, the pH of the system is adjusted to 8, and then tetraethyl orthosilicate and KH550 are added dropwise, and the system temperature is maintained at 30°C, and the reaction is stirred for 4 hours. After the reaction is completed, the filter cake is washed and filtered, and then dispersed in acetone for ultrasonic 30 minutes. After reflux at 80°C for 8 hours, it is washed and filtered, and an equal amount of acetone is added to continue to reflux for 8 hours, and then washed and filtered, and vacuum dried at 60°C for 8 hours to obtain HNTs@MPS nanomaterials. The amount ratio of halloysite nanotubes, hexadecyltrimethylammonium bromide, deionized water, tetraethyl orthosilicate, KH550 and acetone is 1g:2g:200mL:3mL:2.21g:400mL;
[0023] Step A2, stirring and mixing nano titanium dioxide, KH550, ethanol and deionized water in a reactor, raising the system temperature to 40°C, continuing to stir and react for 3 hours, centrifuging and washing after the reaction is completed, re-dispersing the precipitate in acetone for 30 minutes of ultrasound, and controlling the system temperature at 0°C, adding cyanuric chloride and triethylamine, stirring and reacting for 3 hours, and centrifuging, washing and drying after the reaction is completed to obtain modified titanium dioxide, wherein the amount ratio of nano titanium dioxide, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 1g:2.21g:50mL:10mL:100mL:1.84g:1g;
[0024] Step A3, 4-amino-2,6-di-tert-butylphenol and acetone were mixed evenly in a beaker, recorded as solution 1, HNTs@MPS nanomaterials and acetone were mixed evenly in a beaker, recorded as solution 2, modified titanium dioxide and acetone were added to the reactor and mixed evenly, and then solution 1 was slowly added dropwise to the above solution, and the system temperature was controlled to 40°C, and then half of the 0.1 mol / L sodium hydroxide solution was slowly added dropwise, and the reaction was continued for 3 hours, and the system temperature was continued to be raised to 85°C, and then the solution was slowly added dropwise 2 and the remaining sodium hydroxide solution, and the reaction is continued for 5 hours. After the reaction is completed, centrifuge, wash and dry to obtain modified nanomaterials. The dosage ratio of modified titanium dioxide, acetone, solution 1, solution 2 and sodium hydroxide solution is 1g:200mL:20mL:20mL:40mL; the dosage ratio of 4-amino-2,6-di-tert-butylphenol and acetone in solution 1 is 2.21g:20mL, and the dosage ratio of HNTs@MPS nanomaterials and acetone in solution 2 is 1.5g:20mL.
[0025] Example 2
[0026] The modified nanomaterials are prepared by the following steps:
[0027] Step A1, halloysite nanotubes, hexadecyltrimethylammonium bromide and deionized water are mixed in a reactor, and then ultrasonically treated for 45 minutes, the pH of the system is adjusted to 10, and then tetraethyl orthosilicate and KH550 are added dropwise, and the system temperature is maintained at 40°C, and the reaction is stirred for 6 hours. After the reaction is completed, the filter cake is washed and filtered, and then dispersed in acetone for ultrasonication for 30 minutes. After reflux at 90°C for 9 hours, it is washed and filtered, and an equal amount of acetone is added to continue to reflux for 9 hours, and then washed and filtered, and vacuum dried at 60°C for 10 hours to obtain HNTs@MPS nanomaterials. The amount ratio of halloysite nanotubes, hexadecyltrimethylammonium bromide, deionized water, tetraethyl orthosilicate, KH550 and acetone is 1g:3g:200mL:3.5mL:3.32g:400mL;
[0028] Step A2, stirring and mixing nano titanium dioxide, KH550, ethanol and deionized water in a reactor, raising the system temperature to 60°C, continuing to stir and react for 4 hours, centrifuging and washing after the reaction is completed, re-dispersing the precipitate in acetone for 30 minutes of ultrasound, and controlling the system temperature at 0°C, adding cyanuric chloride and triethylamine, stirring and reacting for 4 hours, and centrifuging, washing and drying after the reaction is completed to obtain modified titanium dioxide, the amount ratio of nano titanium dioxide, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 1.5g:3.32g:50mL:10mL:100mL:2.76g:2g;
[0029] Step A3, 4-amino-2,6-di-tert-butylphenol and acetone were mixed evenly in a beaker, recorded as solution 1, HNTs@MPS nanomaterials and acetone were mixed evenly in a beaker, recorded as solution 2, modified titanium dioxide and acetone were added to the reactor and mixed evenly, and then solution 1 was slowly added dropwise to the above solution, and the system temperature was controlled to 45°C, and then half of the 0.1 mol / L sodium hydroxide solution was slowly added dropwise, and the reaction was continued for 3.5 hours, and the system temperature was continued to be raised to 90°C, and then the solution was slowly added dropwise. Liquid 2 and the remaining sodium hydroxide solution are reacted for 6 hours. After the reaction is completed, centrifugation, washing and drying are carried out to obtain modified nanomaterials. The dosage ratio of modified titanium dioxide, acetone, solution 1, solution 2 and sodium hydroxide solution is 1.5g:200mL:20mL:20mL:60mL; the dosage ratio of 4-amino-2,6-di-tert-butylphenol and acetone in solution 1 is 3.32g:20mL, and the dosage ratio of HNTs@MPS nanomaterials and acetone in solution 2 is 2g:20mL.
[0030] Example 3
[0031] The modified nanomaterials are prepared by the following steps:
[0032] Step A1, halloysite nanotubes, hexadecyltrimethylammonium bromide and deionized water are mixed in a reactor, and then ultrasonically treated for 60 minutes, the pH of the system is adjusted to 12, and then tetraethyl orthosilicate and KH550 are added dropwise, and the system temperature is maintained at 50°C, and the reaction is stirred for 8 hours. After the reaction is completed, the filter cake is washed and filtered, and then dispersed in acetone for ultrasonication for 30 minutes. After reflux at 100°C for 10 hours, it is washed and filtered, and an equal amount of acetone is added to continue to reflux for 10 hours, and then washed and filtered, and vacuum dried at 60°C for 12 hours to obtain HNTs@MPS nanomaterials. The amount ratio of halloysite nanotubes, hexadecyltrimethylammonium bromide, deionized water, tetraethyl orthosilicate, KH550 and acetone is 1g:4g:200mL:4mL:4.42g:400mL;
[0033] Step A2, stirring and mixing nano titanium dioxide, KH550, ethanol and deionized water in a reactor, raising the system temperature to 80°C, continuing to stir and react for 5 hours, centrifuging and washing after the reaction is completed, re-dispersing the precipitate in acetone for ultrasonication for 30 minutes, and controlling the system temperature at 5°C, adding cyanuric chloride and triethylamine, stirring and reacting for 5 hours, and centrifuging, washing and drying after the reaction is completed to obtain modified titanium dioxide, wherein the amount ratio of nano titanium dioxide, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 2g:4.42g:50mL:10mL:100mL:3.68g:3g;
[0034] Step A3, 4-amino-2,6-di-tert-butylphenol and acetone were mixed evenly in a beaker, recorded as solution 1, HNTs@MPS nanomaterials and acetone were mixed evenly in a beaker, recorded as solution 2, modified titanium dioxide and acetone were added to the reactor and mixed evenly, and then solution 1 was slowly added dropwise to the above solution, and the system temperature was controlled to 50°C, and then half of the 0.1 mol / L sodium hydroxide solution was slowly added dropwise, and the reaction was continued for 4 hours, and the system temperature was continued to be raised to 95°C, and then the solution was slowly added dropwise 2 and the remaining sodium hydroxide solution, and the reaction is continued for 7 hours. After the reaction is completed, centrifuge, wash and dry to obtain modified nanomaterials. The dosage ratio of modified titanium dioxide, acetone, solution 1, solution 2 and sodium hydroxide solution is 2g:200mL:20mL:20mL:80mL; the dosage ratio of 4-amino-2,6-di-tert-butylphenol and acetone in solution 1 is 4.42g:20mL, and the dosage ratio of HNTs@MPS nanomaterials and acetone in solution 2 is 2.5g:20mL.
[0035] Example 4
[0036] A method for preparing SBS modified asphalt comprises the following steps:
[0037] 100 parts of petroleum asphalt, 3 parts of linear SBS (molecular weight 200,000), 2 parts of modified nanomaterial prepared in Example 1, 0.2 parts of sulfur;
[0038] The raw materials were weighed according to weight fractions, petroleum asphalt was heated to 160° C. and stirred, and then linear SBS, the modified nanomaterial prepared in Example 1 and sulfur were added and stirred and sheared for 2.5 hours to obtain SBS modified asphalt.
[0039] Example 5
[0040] A method for preparing SBS modified asphalt comprises the following steps:
[0041] 100 parts of petroleum asphalt, 5 parts of linear SBS (molecular weight 200,000), 6 parts of modified nanomaterial prepared in Example 2, and 0.6 parts of sulfur;
[0042] The raw materials were weighed according to weight fractions, petroleum asphalt was heated to 170° C. and stirred, and then linear SBS, the modified nanomaterial prepared in Example 2 and sulfur were added and stirred and sheared for 3.5 hours to obtain SBS modified asphalt.
[0043] Example 6
[0044] A method for preparing SBS modified asphalt comprises the following steps:
[0045] 100 parts of petroleum asphalt, 7 parts of linear SBS (molecular weight 200,000), 10 parts of modified nanomaterial prepared in Example 3, 0.8 parts of sulfur;
[0046] The raw materials were weighed according to weight fractions, petroleum asphalt was heated to 180° C. and stirred, and then linear SBS, the modified nanomaterial prepared in Example 3 and sulfur were added and stirred and sheared for 4.5 hours to obtain SBS modified asphalt.
[0047] Comparative Example 1
[0048] This comparative example is an SBS modified asphalt, which differs from Example 6 in that the modified nanomaterial prepared in Example 3 is not added, and the rest is the same.
[0049] Comparative Example 2
[0050] This comparative example is an SBS modified asphalt, which differs from Example 6 in that an equal amount of halloysite nanotubes is used to replace the modified nanomaterial prepared in Example 3, and the rest are the same.
[0051] The SBS modified asphalt prepared in Examples 4-6 and Comparative Examples 1-2 was subjected to performance tests:
[0052] Ductility test: GB / T0605-1993 is used as the experimental standard to test the ductility of the sample at 5°C;
[0053] Anti-aging performance test: Using a film oven test, place the test sample at 163°C for 5 hours, and then test the ductility at 5°C;
[0054] Elastic recovery test: GB / T 0661-1998 is used as the experimental standard. At 25°C, stretch the sample to 10cm at a stretching speed of 5°C / min, cut the sample from the middle, keep the water temperature for 1h, and measure the percentage of recoverable deformation of the sample;
[0055] Segregation test: Based on GB / T 0661-2000 as the experimental standard, place the sample in a 163℃ oven for 48 hours, take the sample at the upper and lower 1 / 3 ends, and test the difference in softening point using the ring and ball method. The test structure is shown in the following table:
[0056]
[0057] It can be seen from the above table that the modified asphalt prepared by the method of the present invention has an ductility of 52-57 cm before the aging test, and after the aging test at 163°C for 5 h, its ductility is still higher than the standard requirement (>15 cm), the elastic recovery rate is in the range of 96.9%-99.3%, and the segregation temperature difference is in the range of 0.2°C-0.5°C; therefore, the modified asphalt of the present invention not only has excellent aging resistance and mechanical properties, but also has good storage stability.
[0058] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A SBS modified asphalt, characterized in that: The raw materials include the following parts by weight: 100 parts of asphalt, 3-7 parts of SBS, 2-10 parts of modified nanomaterials, and 0.2-0.8 parts of stabilizer; The modified nanomaterial is prepared by the following steps: Step A1, mixing halloysite nanotubes, hexadecyltrimethylammonium bromide and deionized water in a reactor, and then ultrasonically treating for 30-60 minutes, adjusting the pH of the system to 8-12, and then adding tetraethyl orthosilicate and KH550 dropwise, and maintaining the system temperature at 30-50° C., stirring and reacting for 4-8 hours, after the reaction is completed, washing and filtering, dispersing the filter cake in acetone and ultrasonicating for 30 minutes, placing it at 80-100° C. and refluxing for 8-10 hours, washing, filtering, adding an equal amount of acetone and continuing to reflux for 8-10 hours, washing, filtering, and vacuum drying at 60° C. for 8-12 hours to obtain HNTs@MPS nanomaterials; Step A2, stirring and mixing nano titanium dioxide, KH550, ethanol and deionized water in a reactor, raising the system temperature to 40-80°C, continuing to stir and react for 3-5 hours, centrifuging and washing after the reaction is completed, re-dispersing the precipitate in acetone and ultrasonicating for 30 minutes, and controlling the system temperature at 0-5°C, adding cyanuric chloride and triethylamine, stirring and reacting for 3-5 hours, and centrifuging, washing and drying after the reaction is completed to obtain modified titanium dioxide; Step A3, 4-amino-2,6-di-tert-butylphenol and acetone are mixed evenly in a beaker, recorded as solution 1, HNTs@MPS nanomaterials and acetone are mixed evenly in a beaker, recorded as solution 2, modified titanium dioxide and acetone are added to a reactor and mixed evenly, then solution 1 is slowly added dropwise to the above solution, and the system temperature is controlled to be 40-50° C., and then half of the 0.1 mol / L sodium hydroxide solution is slowly added dropwise, and the reaction is carried out for 3-4 hours, and the system temperature is continuously raised to 85-95° C., and then solution 2 and the remaining sodium hydroxide solution are slowly added dropwise, and the reaction is continued for 5-7 hours. After the reaction is completed, centrifugation, washing, and drying are performed to obtain the modified nanomaterial; In step A2, the usage ratio of nano-titanium dioxide, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 1-2g: 2.21-4.42g: 50mL: 10mL: 100mL: 1.84-3.68g: 1-3g.
2. The SBS modified asphalt according to claim 1, characterized in that: In step A1, the usage ratio of halloysite nanotubes, hexadecyltrimethylammonium bromide, deionized water, tetraethyl orthosilicate, KH550 and acetone is 1 g: 2-4 g: 200 mL: 3-4 mL: 2.21-4.42 g: 400 mL.
3. The SBS modified asphalt according to claim 1, characterized in that: In step A3, the usage ratio of modified titanium dioxide, acetone, solution 1, solution 2 and sodium hydroxide solution is 1-2 g: 200 mL: 20 mL: 20 mL: 40-80 mL.
4. The SBS modified asphalt according to claim 3, characterized in that: The dosage ratio of 4-amino-2,6-di-tert-butylphenol and acetone in solution 1 is 2.21-4.42 g: 20 mL.
5. The SBS modified asphalt according to claim 3, characterized in that: The dosage ratio of HNTs@MPS nanomaterials and acetone in solution 2 is 1.5-2.5 g: 20 mL.
6. The method for preparing SBS modified asphalt according to claim 1, characterized in that: The following steps are involved: Weigh the raw materials according to the weight fraction, heat the asphalt to 160-180°C, stir, then add SBS, modified nanomaterials and stabilizer, stir and shear for 2.5-4.5 hours to obtain SBS modified asphalt.