A low-density and high-thermal-conductivity two-component polyurethane structural adhesive and preparation method thereof

By using modified flake mineral powder and nano-silica powder in polyurethane structural adhesive, the problem of insufficient thermal conductivity and bonding strength of low-density polyurethane structural adhesive is solved, and a low-density polyurethane structure with high thermal conductivity and strong bonding is achieved. Glue, suitable for heat dissipation and bonding applications of electronic components.

CN118185541BActive Publication Date: 2024-10-29GOLOHO POLYMER (JIANGXI) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410375273.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-29
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing polyurethane structural adhesives have low thermal conductivity and bonding strength at low density, making it difficult to meet the heat dissipation and bonding needs of electronic components.

Method used

Modified flaky mineral powder is used as the thixotropic agent to form a dynamic cross-linked network through surface chemical grafting to improve the dispersion uniformity and stability of the thermally conductive powder, and is combined with nano-silica powder to enhance the thermal conductivity path and mechanical properties.

Benefits of technology

It has improved the stability and thermal conductivity of low-density and high thermal conductivity two-component polyurethane structural adhesive, enhanced bonding strength and mechanical properties, and is suitable for heat dissipation and bonding applications of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004766863370000081
    Figure BDA0004766863370000081
  • Figure BDA0004766863370000091
    Figure BDA0004766863370000091
Patent Text Reader

Abstract

The present invention relates to the field of polyurethane structural adhesive, and more particularly to a low-density high-thermal-conductivity two-component polyurethane structural adhesive and a preparation method thereof, wherein the structural adhesive comprises component A and component B, wherein the component A comprises 20% to 40% of polyol, 50% to 70% of thermally conductive powder, 1% to 10% of water absorbent, 0.01% to 0.5% of thixotropic agent and 0.1% to 1% of dispersant by weight percentage; wherein the thixotropic agent comprises modified flaky mineral powder, the particle size of the modified flaky mineral powder being 100-325 mesh; and the surface chemical grafting of the modified flaky mineral powder is useful for generating hydrogen bond acceptor segments of a dynamic cross-linked network with polyol. The present invention has better bonding ability than the prior art, can firmly bond metal and plastic products, and due to the addition of self-compounded powder with thixotropic properties, it has good anti-settling performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyurethane structural adhesives, and in particular to a low-density and high-thermal-conductivity two-component polyurethane structural adhesive and a preparation method thereof. Background Art

[0002] Polyurethane structural adhesive has excellent mechanical properties and processing properties, anti-corrosion and waterproof, good insulation and other characteristics, and is widely used in the fields of sealing and bonding. Polyurethane structural adhesive is used for bonding plastics and metals, and needs to have good bonding ability and sealing. It is widely used in the field of electronic appliances, mainly for heat dissipation and protection of electronic components, which requires it to have a small density, good mechanical properties, bonding properties and good thermal conductivity after curing, and it must not corrode the components of the electronic circuit board.

[0003] With the development of the electronics industry, the size of internal components of electronic equipment has been reduced, and the internal working environment temperature has continued to rise. Therefore, the thermal conductivity of polyurethane structural adhesives has also become a research hotspot.

[0004] For example: A Chinese patent document with publication number CN202211647373, publication date December 21, 2022, and titled "Low-density high-thermal-conductivity polyurethane potting adhesive and preparation method thereof" discloses a method for preparing a polyurethane potting adhesive. The present invention belongs to the technical field of polyurethane potting adhesives, and specifically relates to a low-density high-thermal-conductivity polyurethane potting adhesive and a preparation method thereof. The invention has the characteristics of low density and high thermal conductivity. However, it should be pointed out that, although the technical solution disclosed in the patent document can achieve low-density and high-thermal-conductivity performance, the potting adhesive has poor bonding ability and is not suitable for bonding materials such as metals and electronic components.

[0005] Another example: The invention described in the Chinese patent document with publication number CN202310810744 and publication date September 12, 2023, entitled “A high thermal conductivity, detachable polyurethane structural adhesive and its preparation method” belongs to the field of high thermal conductivity polyurethane structural adhesive, and specifically relates to a high thermal conductivity, detachable polyurethane structural adhesive and its preparation method. The polyurethane structural adhesive includes component A and component B. The present invention uses a structural controller and an inhibitor in the polyurethane structural adhesive, which can effectively improve the detachability of the polyurethane structural adhesive while ensuring that the polyurethane structural adhesive has a good bonding effect, and at the same time control the curing rate of the polyurethane structural adhesive, thereby gaining more fault tolerance time for actual operation. However, this high thermal conductivity structural adhesive has a high density, and the thermal conductive filler is prone to stratification during storage. At the same time, it is brittle after curing and is prone to cracking during use.

[0006] Based on the above, it can be seen that the prior art lacks an effective method to achieve high thermal conductivity and good bonding strength at low density. Therefore, it is necessary to modify the traditional polyurethane structural adhesive to improve the thermal conductivity and bonding performance of polyurethane. Summary of the invention

[0007] The present invention aims to overcome the defects of low thermal conductivity and low bonding strength of low-density polyurethane structural adhesive in the prior art, and provides a low-density and high-thermal-conductivity two-component polyurethane structural adhesive and a preparation method thereof to overcome the above-mentioned shortcomings.

[0008] To achieve the above-mentioned purpose, the present invention is implemented by the following technical solutions:

[0009] In a first aspect, the present invention first provides a low-density and high-thermal-conductivity two-component polyurethane structural adhesive, comprising component A and component B;

[0010] The component A comprises, by weight percentage, 20% to 40% of polyol, 50% to 70% of thermal conductive powder, 1% to 10% of water absorbent, 0.01% to 0.5% of thixotropic agent and 0.1% to 1% of dispersant;

[0011] The component B comprises, by weight percentage, 10% to 30% of isocyanate, 10% to 20% of plasticizer, 50% to 60% of flame retardant, 1% to 10% of defoamer and 0.1% to 10% of catalyst;

[0012] The thixotropic agent comprises modified flaky mineral powder, the particle size of the modified flaky mineral powder is 100-325 meshes; and the surface of the modified flaky mineral powder is chemically grafted with hydrogen bond receptor segments for generating a dynamic cross-linking network with polyols.

[0013] The low-density high-thermal-conductivity two-component polyurethane structural adhesive of the present invention contains a relatively high content of thermally conductive powder, so that the prepared low-density high-thermal-conductivity two-component polyurethane structural adhesive has good thermal conductivity. However, as the amount of thermally conductive powder added increases, the thermally conductive powder will agglomerate and settle during storage of the two-component polyurethane structural adhesive, thereby causing the two-component polyurethane structural adhesive to have a reduced ease of use and performance during use.

[0014] In order to prevent the above defects, the present application creatively proposes the use of modified flaky mineral powder as a thixotropic agent, thereby improving the performance of the two-component polyurethane structural adhesive in terms of preventing sedimentation, improving thermal conductivity and improving bonding strength.

[0015] First, the present invention selects modified flaky mineral powder as a thixotropic agent. Since the modified flaky mineral powder has a lamellar structure, when the modified flaky mineral powder is dispersed in component A of the polyurethane structural adhesive, a large amount of space for accommodating components such as polyols and thermal conductive powder will be formed between the modified flaky mineral powders, so that these components can be adsorbed by the modified flaky mineral powder, thereby greatly improving the stability of component A.

[0016] At the same time, since the surface of the modified flaky mineral powder is chemically grafted with hydrogen bond acceptor segments that are used to produce a dynamic cross-linked network with polyols, after component A is formulated, there are a large number of unstable cross-linked networks composed of hydrogen bonds in component A of the two-component polyurethane structural adhesive, thereby further locking the dispersion uniformity and stability of each raw material in component A.

[0017] At the same time, these unstable cross-linked networks formed by hydrogen bonds can be destroyed under the action of external force, thereby reducing the difficulty of mixing component A and component B. When the external force disappears, these unstable cross-linked networks formed by hydrogen bonds will be re-formed, thereby maintaining the stability of the two-component polyurethane structural adhesive.

[0018] In addition, due to the effective improvement of the dispersion uniformity and stability of each raw material in component A, the thermal conductivity path formed by the interconnected thermal conductive powder can be effectively maintained and stabilized, so the thermal conductivity path can be kept stable, thereby improving the thermal conductivity of the two-component polyurethane structural adhesive. At the same time, since the modified flaky mineral powder itself also has good thermal conductivity, when it is also involved in the establishment of the thermal conductivity path of the two-component polyurethane structural adhesive, the thermal conductivity effect of the two-component polyurethane structural adhesive can be further improved.

[0019] In addition, since the unstable cross-linking network composed of hydrogen bonds in the two-component polyurethane structural adhesive can remain stable after curing, its bonding strength can be effectively improved.

[0020] Finally, the applicant found that the particle size of the modified flaky mineral powder has a greater impact on the performance of the two-component polyurethane structural adhesive. When the particle size of the modified flaky mineral powder is too large, the weight of the modified flaky mineral powder itself is large, so its own anti-sedimentation performance is poor, and it is easy to settle during storage. When the particle size of the modified flaky mineral powder is too small, the aggregation of the modified flaky mineral powder itself will be greatly improved, so it is easy to agglomerate, causing the failure of the cross-linked network. Therefore, after comprehensive consideration by the applicant, when the particle size of the modified flaky mineral powder is within the range of 100-325 mesh, it can effectively guarantee the comprehensive performance of the low-density and high-thermal-conductivity two-component polyurethane structural adhesive in this application.

[0021] Preferably, the preparation method of the modified flaky mineral powder is as follows:

[0022] - placing the flaky mineral powder in a silane coupling agent solution containing a silicon-hydrogen structure, and hydrolyzing the silane coupling agent so that the silane coupling agent couples on the surface of the flaky mineral powder to form a coupling layer containing a silicon-hydrogen structure;

[0023] - subjecting the flaky mineral powder having a coupling layer on its surface to a hydrosilylation reaction with a compound having both a hydrogen bond acceptor group and an unsaturated group, thereby obtaining the modified flaky mineral powder.

[0024] In the preparation process of the modified flaky mineral powder of the present application, a coupling layer is formed on the surface of the flaky mineral powder by the silicon-hydrogen coupling agent. The formation of the coupling layer can enhance the compatibility of the flaky mineral powder with other components in the system, which is beneficial to improving the dispersibility of the flaky mineral powder in the structural adhesive.

[0025] At the same time, after the silicon-hydrogen coupling agent forms a coupling layer with the surface of the flaky mineral powder, the coupling layer has a silicon-hydrogen structure and can undergo a silicon-hydrogen addition reaction with a compound containing a hydrogen bond acceptor group and an unsaturated group. This reaction chemically grafts a hydrogen bond acceptor segment on the surface of the modified flaky mineral powder that can produce a dynamic cross-linking network with the polyol, which helps to improve its ability to interact with the polyol, thereby improving the adhesion of the modified flaky mineral powder in the structural adhesive.

[0026] In addition, the chemical properties of the surface of the modified flaky mineral powder have changed, which has a positive effect on the thermal conductivity. Through chemical modification, the surface morphology and chemical properties of the modified flaky mineral powder are more suitable for the thermal conductivity requirements of the structural adhesive, improving the overall thermal conductivity of the structural adhesive.

[0027] Finally, the improved chemical properties and surface characteristics of the modified flake mineral powder may improve its stability in structural adhesives, reduce the possibility of sedimentation and phase separation, and extend the service life of the structural adhesive.

[0028] Preferably, the flaky mineral powder is any one of mica powder, talc powder and montmorillonite;

[0029] The silane coupling agent is any one of trimethoxysilane, triethoxysilane, methyldimethoxysilane and methyldiethoxysilane.

[0030] Preferably, the compound containing both a hydrogen bond acceptor group and an unsaturated group is any one of acrylamide, hydroxyethyl acrylate and N-vinyl pyrrolidone.

[0031] Preferably, the thixotropic agent further comprises nano silicon dioxide powder in an amount not higher than 150% of the mass of the flaky mineral powder.

[0032] Nano-silica powder has a large specific surface area and high activity. Adding it to structural adhesive can fill tiny gaps and cracks, enhancing the filling effect of structural adhesive. This helps to improve the density and uniformity of structural adhesive, which is beneficial to improving the mechanical properties of the product.

[0033] At the same time, the addition of nano-silica powder can form multiple heat conduction paths in the structural adhesive, which is beneficial to improve the overall thermal conductivity of the structural adhesive. This effect can make the structural adhesive more effective in dispersing and transferring heat, which helps to improve the performance of thermal conductive materials in applications that require heat dissipation and heat conduction.

[0034] In addition, since nano-silica powder has good toughening and thickening effects, its addition helps to improve the mechanical strength and wear resistance of structural adhesives. This helps to increase the service life and durability of the product. Moreover, it can change the surface properties of structural adhesives, which has a certain positive effect on improving its adhesion performance with other materials, and helps to improve the use effect of the product.

[0035] However, the inventors of the present application discovered during the experiment that the amount of nano-silica powder added has an important impact on the low-density, high-thermal-conductivity two-component polyurethane structural adhesive in the present application. The inventors found that adding too high a proportion of silica powder may significantly change the rheological properties of the structural adhesive, increasing its viscosity and making it more difficult to adjust, which will bring challenges to the production process. At the same time, adding silica powder in a high proportion may lead to the opposite effect, thereby making the composition of the structural adhesive unstable, causing phase separation or deposition, reducing the uniformity and stability of the product, reducing the overall thermal conductivity of the structural adhesive, and affecting its performance in applications requiring thermal conductivity.

[0036] Preferably, the polyol is one or a mixture of polyester polyols, polyether polyols, bio-based polyols, aromatic polyols, polyolefin polyols, castor oil, modified castor oil, palm oil, and soybean oil with a molecular weight of 400 to 4000 and a functionality of 2 to 4.

[0037] Preferably, the thermally conductive powder comprises: one or a mixture of aluminum oxide, magnesium oxide, aluminum hydroxide, copper oxide, boron nitride and zinc oxide;

[0038] The water absorbent includes one or more composites of molecular sieves such as aluminosilicate molecular sieve, titanium silicon molecular sieve, ZSM-35 molecular sieve, ZSM-5 molecular sieve, CR-500 molecular sieve, etc.;

[0039] The dispersant includes any one of a wetting dispersant, a polyurethane dispersant, and a polyacrylic acid dispersant.

[0040] Preferably, the isocyanate is an isocyanate with a functionality of 2-4, comprising one or more mixtures of liquefied MDI-2020, liquefied MDI-50, isocyanate 9258, isocyanate PM-200, isocyanate 2642, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, p-phenylene diisocyanate, 1,4-cyclohexane diisocyanate, cyclohexane dimethylene diisocyanate, trimethyl-1,6-hexamethylene diisocyanate, dimethyl biphenyl diisocyanate, methylcyclohexyl diisocyanate, dimethyl diphenylmethane diisocyanate, and lysine diisocyanate;

[0041] The plasticizer includes one or more of paraffin, asphalt, plasticizer DOP and plasticizer DIDP;

[0042] The flame retardant includes any one of a halogen flame retardant, a phosphorus flame retardant and an inorganic flame retardant;

[0043] The defoaming agent includes an organosilicon defoaming agent from AFCONA;

[0044] The catalyst includes one or more complexes of amine catalysts, organic zinc catalysts, organic bismuth catalysts, titanate catalysts and the like.

[0045] In a second aspect, the present invention further provides a method for preparing the low-density and high-thermal-conductivity two-component polyurethane structural adhesive, comprising the following steps:

[0046] (S.1) placing polyol, thermal conductive powder, water absorbent, thixotropic agent and dispersant in a vacuum stirring degassing machine according to a proportion and mixing to obtain component A;

[0047] (S.2) mixing isocyanate, plasticizer, flame retardant, defoamer and catalyst in a vacuum stirring degassing machine according to a proportion to obtain component B;

[0048] (S.3) Mixing component A and component B by vacuum degassing and coating to obtain the low-density and high-thermal-conductivity two-component polyurethane structural adhesive.

[0049] Preferably, the rotation speed of the vacuum stirring degassing machine in step (S.1) and step (S.2) is 2000-4000 rad / min, and the degassing time is 2-6 min.

[0050] Therefore, compared with the prior art, the present invention has the following beneficial effects:

[0051] (1) The polyurethane structural adhesive has a low density. When bonding electronic components, it makes the electronic products light and easy to carry. It has good thermal conductivity and plays a role in heat dissipation and protection for electronic components.

[0052] (2) The polyurethane structural adhesive has good bonding ability and can firmly bond metal and plastic products. After curing, the bonding force is even stronger and can even be applied to more places and fields;

[0053] (3) The polyurethane structural adhesive is added with self-compounded powder with thixotropic properties, has good anti-settling performance, is easy to disperse, simple to operate, and has little wear on equipment;

[0054] (4) In addition, the polyurethane structural adhesive has good mechanical properties, strong tensile strength and low hardness. During use, it is easy to operate and is non-toxic and pollution-free. DETAILED DESCRIPTION

[0055] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.

[0056]

Preparation of modified flaky mineral powder

[0057] Modified flake mineral powder A:

[0058] Step (1): placing 100 g of muscovite powder (100 mesh) in 500 ml of a 70% ethanol aqueous solution containing trimethoxysilane at a concentration of 10 g / L, adjusting the pH of the solution to 5, and stirring the solution at 40° C. for 3 h to allow the trimethoxysilane to condense on the surface of the muscovite powder to form a coupling layer containing a silicon-hydrogen structure. After the reaction is completed, the mixture is washed with anhydrous ethanol to obtain a muscovite powder having a coupling layer on the surface;

[0059] Step (2): The muscovite powder having a coupling layer on the surface prepared in step (1) is dispersed in 500 ml of toluene, and 11.6 g (0.1 mol) of hydroxyethyl acrylate and 10 mg of Custer catalyst are added to the solution. The mixture is refluxed for 3 hours to cause a hydrosilylation reaction. After the reaction is completed, the mixture is filtered and the filter residue is washed with anhydrous ethanol to obtain a modified flaky mineral powder A.

[0060] Modified flake mineral powder B:

[0061] Step (1): placing 100 g of muscovite powder (200 mesh) in 500 ml of a 70% ethanol aqueous solution containing methyldimethoxysilane at a concentration of 10 g / L, adjusting the pH of the solution to 5, and stirring the solution at 50° C. for 2.5 hours to allow methyldimethoxysilane to condense on the surface of the muscovite powder to form a coupling layer containing a silicon-hydrogen structure. After the reaction is completed, the mixture is washed with anhydrous ethanol to obtain a muscovite powder having a coupling layer on the surface;

[0062] Step (2): The muscovite powder having a coupling layer on the surface prepared in step (1) is dispersed in 500 ml of toluene, and 7.1 g (0.1 mol) of acrylamide and 10 mg of Custer catalyst are added to the solution. The mixture is refluxed for 3 hours to cause a hydrosilylation reaction. After the reaction is completed, the mixture is filtered and the filter residue is washed with anhydrous ethanol to obtain a modified flaky mineral powder B.

[0063] Modified flake mineral powder C:

[0064] Step (1): placing 100 g of montmorillonite (325 mesh) in 500 ml of a 70% ethanol aqueous solution containing methyldimethoxysilane at a concentration of 20 g / L, adjusting the solution pH to 5, and stirring at 50° C. for 3 h to allow methyldimethoxysilane to condense on the surface of the montmorillonite to form a coupling layer containing a silicon-hydrogen structure. After the reaction is completed, washing is performed with anhydrous ethanol to obtain a montmorillonite having a coupling layer on the surface;

[0065] Step (2): The montmorillonite having a coupling layer on its surface prepared in step (1) is dispersed in 500 ml of toluene, and 16.6 g (0.1 mol) of furfuryl methacrylate and 10 mg of Custer catalyst are added to the solution. The mixture is refluxed for 3 hours to cause a hydrosilylation reaction. After the reaction is completed, the mixture is filtered and the filter residue is washed with anhydrous ethanol to obtain a modified flaky mineral powder C.

[0066] Modified flake mineral powder D:

[0067] The preparation method of modified flaky mineral powder D is the same as that of modified flaky mineral powder A, except that muscovite powder (100 mesh) is replaced by muscovite powder (50 mesh).

[0068] Modified flake mineral powder E:

[0069] The preparation method of the modified flaky mineral powder E is the same as that of the modified flaky mineral powder A, except that the muscovite powder (100 mesh) is replaced by muscovite powder (500 mesh).

[0070] Example 1

[0071] A low-density and high-thermal-conductivity two-component polyurethane structural adhesive, the preparation method of which comprises the following steps:

[0072] Step S1: Component A is prepared according to the following preparation method: 30 parts of polyol H368 with a molecular weight of 400-3000, a hydroxyl value of 30-300 mgKOH / g, and a functionality of 2-3.5, 59 parts of alumina powder, 10 parts of aluminosilicate molecular sieves, 0.5 parts of modified flaky mineral powder A and 0.5 parts of polyurethane dispersant SRE-4026 are mixed, and degassing is performed for 5 minutes at a speed of 3000 rad / min using a vacuum stirring degassing machine to obtain component A.

[0073] Step S2: 20 parts of isocyanate liquefied MDI, 15 parts of plasticizer DIDP, 55 parts of flame retardant FRV-188, 5 parts of defoamer 2620 and 5 parts of catalyst AS11 are mixed, and defoamed for 5 minutes at a speed of 2000-4000 rad / min using a vacuum stirring degassing machine to obtain component A.

[0074] Step S3: Mix component A and component B in a ratio of 1:1-2 by vacuum degassing, apply film, and observe the surface drying time and curing time.

[0075] Example 2-3

[0076] The difference between Example 2 and Example 3 and Example 1 is that the modified flaky mineral powder A in Example 1 is replaced by modified flaky mineral powder B and modified flaky mineral powder C respectively.

[0077] Embodiment 4-5

[0078] The difference between Example 4 and Example 5 and Example 1 is that, on the basis of Example 1, 0.5 parts and 0.75 parts of nano silicon dioxide powder are added respectively.

[0079] Example 6

[0080] A low-density and high-thermal-conductivity two-component polyurethane structural adhesive, the preparation method of which comprises the following steps:

[0081] Step S1: Component A is prepared according to the following preparation method: 20 parts of castor oil, 70 parts of aluminum oxide powder, 8 parts of aluminum silicate molecular sieve, 1 part of modified flaky mineral powder C and 1 part of polyurethane dispersant SRE-4026 are mixed, and degassing time is 6 minutes at a speed of 2000 rad / min using a vacuum stirring degassing machine to obtain component A.

[0082] Step S2: 15 parts of isocyanate liquefied MDI, 20 parts of plasticizer DOP, 50 parts of flame retardant FRV-188, 10 parts of defoamer 2620 and 5 parts of catalyst AS11 are mixed, and defoamed for 2 minutes at a speed of 4000 rad / min using a vacuum stirring degassing machine to obtain component B.

[0083] Step S3: Mix component A and component B in a ratio of 1:2 by vacuum degassing, apply film, and observe the surface drying time and curing time.

[0084] Example 7

[0085] A low-density and high-thermal-conductivity two-component polyurethane structural adhesive, the preparation method of which comprises the following steps:

[0086] Step S1: Component A is prepared according to the following preparation method: 40 parts of polyether polyol DDL-1000D, 50 parts of alumina powder, 9 parts of aluminosilicate molecular sieve, 0.5 parts of modified flaky mineral powder C and 0.5 parts of polyurethane dispersant SRE-4026 are mixed, and degassing time is 6 minutes at a speed of 2000 rad / min using a vacuum stirring degassing machine to obtain component A.

[0087] Step S2: 30 parts of isocyanate liquefied MDI, 10 parts of plasticizer DOP, 50 parts of flame retardant FRV-188, 1 part of defoamer 2620 and 9 parts of catalyst AS11 are mixed, and defoamed for 2 minutes at a speed of 4000 rad / min using a vacuum stirring degassing machine to obtain component B.

[0088] Step S3: Mix component A and component B in a ratio of 1:2 by vacuum degassing, apply film, and observe the surface drying time and curing time.

[0089] Example 8

[0090] A low-density and high-thermal-conductivity two-component polyurethane structural adhesive, the preparation method of which comprises the following steps:

[0091] Step S1: Component A is prepared according to the following preparation method: 35 parts of polyether polyol DDL-1000D, 62 parts of alumina powder, 1 part of aluminosilicate molecular sieve, 1 part of modified flaky mineral powder C and 1 part of polyurethane dispersant SRE-4026 are mixed, and degassing time is 6 minutes at a speed of 2000 rad / min using a vacuum stirring degassing machine to obtain component A.

[0092] Step S2: 10 parts of isocyanate liquefied MDI-2020, 15 parts of plasticizer DOP, 60 parts of flame retardant FRV-188, 7 parts of defoamer 2620 and 8 parts of catalyst AS11 are mixed, and defoamed for 2 minutes at a speed of 4000 rad / min using a vacuum stirring degassing machine to obtain component B.

[0093] Step S3: Mix component A and component B in a ratio of 1:2 by vacuum degassing, apply film, and observe the surface drying time and curing time.

[0094] Comparative Example 1

[0095] The difference between Comparative Example 1 and Example 1 is that the modified flaky mineral powder A in Example 1 is replaced with unmodified muscovite powder in sequence.

[0096] Comparative Examples 2-3

[0097] The difference between Comparative Examples 2 and 3 and Example 1 is that the modified flaky mineral powder A in Example 1 is replaced by modified flaky mineral powder D and modified flaky mineral powder E respectively.

[0098] Comparative Example 4

[0099] The difference between Comparative Example 4 and Example 1 is that, on the basis of Example 1, 1 portion of nano silicon dioxide powder is additionally added.

[0100] The low-density and high-thermal-conductivity two-component polyurethane structural adhesives prepared in Examples 1 to 8 and Comparative Examples 1 to 4 were tested, and the test results are shown in Table 1 below.

[0101] Table 1

[0102]

[0103]

[0104] From the above experimental results, we can know that the low-density and high-thermal-conductivity two-component polyurethane structural adhesive prepared by the method in this application has higher stability of each component, and there will be no problem of flocculation and sedimentation during storage. At the same time, because the flaky mineral powder is modified, it can maintain the cross-linked network of the structural adhesive and the stable formation of the heat-conducting channel, so that its mechanical properties and thermal conductivity can be significantly improved. In addition, it can be known from the above results that the particle size of the modified flaky mineral powder also has a certain influence on the polyurethane structural adhesive. When the particle size of the modified flaky mineral powder is too large, the weight of the modified flaky mineral powder itself is large, so its own anti-sedimentation performance is poor, and it is easy to settle during storage. When the particle size of the modified flaky mineral powder is too small, the aggregation of the modified flaky mineral powder itself will be greatly improved, so it is also easy to agglomerate, resulting in the failure of the cross-linked network.

[0105] Finally, the inventors of this application discovered during the experiment that the amount of nano-silica powder added has a certain effect on the low-density, high-thermal-conductivity two-component polyurethane structural adhesive in this application. The inventors found that adding too high a proportion of silica powder may significantly change the rheological properties of the structural adhesive, increasing its viscosity and making it more difficult to adjust, which will bring challenges to the production process. At the same time, adding silica powder in a high proportion may lead to the opposite effect, thereby making the composition of the structural adhesive unstable, causing phase separation or deposition, reducing the uniformity and stability of the product, reducing the overall thermal conductivity of the structural adhesive, and affecting its performance in applications requiring thermal conductivity.

[0106] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but this will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.

Claims

1. A low-density, high-thermal-conductivity two-component polyurethane structural adhesive, characterized in that: It contains component A and component B; The component A comprises, by weight percentage, 20% to 40% of polyol, 50% to 70% of thermal conductive powder, 1% to 10% of water absorbent, 0.5% to 1% of thixotropic agent and 0.5% to 1% of dispersant; The component B comprises, by weight percentage, 10% to 30% of isocyanate, 10% to 20% of plasticizer, 50% to 60% of flame retardant, 1% to 10% of defoamer and 5% to 10% of catalyst; Wherein, the thixotropic agent is composed of modified flaky mineral powder and nano-silicon dioxide powder, the mass of the nano-silicon dioxide powder is not higher than 150% of the mass of the modified flaky mineral powder, and the particle size of the modified flaky mineral powder is 100-325 mesh; and, The surface of the modified flaky mineral powder is chemically grafted with hydrogen bond acceptor segments for generating a dynamic cross-linking network with polyols; The preparation method of the modified flaky mineral powder is as follows: - placing the flaky mineral powder in a silane coupling agent solution containing a silicon-hydrogen structure, and hydrolyzing the silane coupling agent so that the silane coupling agent couples on the surface of the flaky mineral powder to form a coupling layer containing a silicon-hydrogen structure; - subjecting the flaky mineral powder having a coupling layer on its surface to a hydrosilylation reaction with a compound having both a hydrogen bond acceptor group and an unsaturated group, thereby obtaining the modified flaky mineral powder; The flaky mineral powder is any one of mica powder, talc powder and montmorillonite; The silane coupling agent is any one of trimethoxysilane, triethoxysilane, methyldimethoxysilane and methyldiethoxysilane; The compound containing both hydrogen bond acceptor groups and unsaturated groups is any one of acrylamide, hydroxyethyl acrylate and N-vinyl pyrrolidone.

2. A low-density, high-thermal-conductivity two-component polyurethane structural adhesive according to claim 1, characterized in that: The polyol is one or a mixture of polyester polyol, polyether polyol, bio-based polyol, aromatic polyol, polyolefin polyol, castor oil, modified castor oil, palm oil, and soybean oil with a molecular weight of 400-4000 and a functionality of 2-4.

3. The low-density and high-thermal-conductivity two-component polyurethane structural adhesive according to claim 1, characterized in that: The thermally conductive powder comprises: one or a mixture of aluminum oxide, magnesium oxide, aluminum hydroxide, copper oxide, boron nitride and zinc oxide; The water absorbent includes one or more composites of aluminosilicate molecular sieve, titanium silicon molecular sieve, ZSM-35 molecular sieve, ZSM-5 molecular sieve, and CR-500 molecular sieve; The dispersant includes any one of a wetting dispersant, a polyurethane dispersant, and a polyacrylic acid dispersant.

4. The low-density and high-thermal-conductivity two-component polyurethane structural adhesive according to claim 1, characterized in that: The isocyanate is an isocyanate with a functionality of 2-4, comprising one or more of liquefied MDI-2020, liquefied MDI-50, isocyanate 9258, isocyanate PM-200, isocyanate 2642, dicyclohexylmethane diisocyanate, naphthalene diisocyanate, p-phenylene diisocyanate, 1,4-cyclohexane diisocyanate, cyclohexane dimethylene diisocyanate, trimethyl-1,6-hexamethylene diisocyanate, dimethyl biphenyl diisocyanate, methyl cyclohexyl diisocyanate, dimethyl diphenylmethane diisocyanate, and lysine diisocyanate; The plasticizer includes one or more of paraffin, asphalt, plasticizer DOP and plasticizer DIDP; The flame retardant includes any one of a halogen flame retardant, a phosphorus flame retardant and an inorganic flame retardant; The defoaming agent includes an organosilicon defoaming agent from AFCONA; The catalyst comprises one or more composites of amine catalysts, organic zinc catalysts, organic bismuth catalysts and titanate catalysts.

5. A method for preparing the low-density and high-thermal-conductivity two-component polyurethane structural adhesive as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: (S.1) Mixing polyol, thermal conductive powder, water absorbent, thixotropic agent and dispersant in a vacuum stirring degassing machine according to a proportion to obtain component A; (S.2) isocyanate, plasticizer, flame retardant, defoamer and catalyst are placed in a vacuum stirring degassing machine according to the proportions and mixed to obtain component B; (S.3) Mixing component A and component B by vacuum degassing and coating to obtain the low-density and high-thermal-conductivity two-component polyurethane structural adhesive.

6. The method according to claim 5, characterized in that In the step (S.1) and the step (S.2), the rotation speed of the vacuum stirring degassing machine is 2000-4000 rad / min, and the degassing time is 2-6 min.

Citation Information

Patent Citations

  • Low-density, high thermal conductivity polyurethane potting compound and its preparation method

    CN115651596B

  • High-thermal-conductivity detachable polyurethane structural adhesive and preparation method thereof

    CN116731660A

  • Specific papermaking filling and paper containing same

    CN103374854A

  • High-elongation anti-sagging polyurethane waterproof coating and preparation method thereof

    CN111909611A