A method for preparing a biomass / metal-organic framework (MOFs) sodium ion battery negative electrode material
By combining natural biomass with a metal-organic framework, excellent sodium ion battery negative electrode material is prepared, which solves the problem of insufficient performance of sodium ion battery, achieves high specific capacity and cycle stability, and is suitable for energy storage and conversion fields.
Patent Information
- Application Number
- CN202410415076.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-08
AI Technical Summary
Due to the large Na+ radius and high ionization potential, existing sodium ion batteries have challenges in cycling stability, capacity maintenance, energy efficiency and rate performance, and lack suitable sodium ion battery anode materials.
By combining natural biomass with metal-organic frameworks (MOFs), porous carbon nanofiber membranes are prepared by high-voltage electrospinning technology, and ZIF-67 is used as a cobalt-based metal organic framework with high conductivity and controllable pore structure to carbonize Treatment to prepare a biomass/metal-organic framework sodium ion battery negative electrode material with excellent electrochemical properties.
It significantly improves the electrochemical performance and cyclic stability of sodium ion batteries, provides improvements in specific capacity and rate performance, overcomes the problems of limited conductivity and specific surface area of traditional hard carbon materials, and achieves efficient energy storage and conversion.
Smart Images

Figure CN118231623B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sodium ion batteries, and relates to a biomass sodium ion battery negative electrode material and a preparation method thereof, and in particular to a method for preparing a high-performance sodium ion battery by combining biomass with metal-organic frameworks (MOFs). Background Art
[0002] With the continuous increase in energy demand and the worsening of environmental problems, the development of sustainable, environmentally friendly, high-performance new energy storage materials has become a huge challenge and opportunity. As a new type of rechargeable battery, sodium-ion batteries have the advantages of high energy density, low cost and wide resource availability. However, the existing sodium-ion batteries have a large number of advantages due to the Na + Due to the large radius and high ionization potential, there are still challenges in terms of cycle stability, capacity retention, energy efficiency and rate performance, and there is a lack of suitable anode materials for sodium-ion batteries. Therefore, a method to improve the performance of sodium-ion batteries is urgently needed to overcome the current limitations.
[0003] Natural biomass materials are widely available, low-cost, environmentally friendly, and form carbonaceous structural characteristics after carbonization. Therefore, they are regarded as a very promising negative electrode material. However, the conductivity and specific surface area of biomass hard carbon materials are limited, and the theoretical capacity is not high. For example, the invention patent application with publication number CN110719891A provides a biomass-based sodium ion battery hard carbon negative electrode material and its preparation method and application. This solution requires the use of permanganate in the preparation process, which is not environmentally friendly, and the capacity and cycle performance of the hard carbon material need to be improved; the invention patent application with publication number CN 116553515 A provides a method for regulating the first charge and discharge coulomb efficiency of a corn stalk-based hard carbon negative electrode and a sodium ion battery. The hard carbon first charge and discharge coulomb efficiency obtained by the provided control strategy based on the heating rate of biomass corn stalks is as high as 87%, and the specific capacity is 304mAh / g, and the efficiency needs to be improved. Summary of the invention
[0004] In order to prepare sustainable, green and high-performance energy storage materials, the purpose of the present invention is to introduce metal-organic frameworks (MOFs) in different ways on biomass-based porous carbon nanofiber materials and combine them with high-temperature carbonization technology to obtain a biomass / metal-organic framework (MOFs) sodium ion battery negative electrode material with excellent electrochemical properties.
[0005] In order to achieve the above objectives, the present invention provides the following technical solutions:
[0006] A method for preparing a biomass / metal-organic framework (MOFs) sodium ion battery negative electrode material comprises the following steps:
[0007] (1) Preparation of ZIF-67 powder;
[0008] (2) Preparing a biomass porous nanofiber composite membrane: preparing an 8 wt% cellulose spinning solution; preparing a 6 wt% chitosan spinning solution, and then mixing the dissolved cellulose and chitosan in a mass ratio of 2:8 to 8:2 to form a mixed solution, adding ZIF-67 powder to the mixed solution to prepare a concentration of 2 to 4 wt% ZIF-67, stirring evenly to obtain a spinning solution, spinning using a high-voltage electrospinning device to obtain a nanofiber composite membrane, and washing and drying the nanofiber composite membrane for later use;
[0009] (3) Preparation of biomass porous carbon nanofiber composite membrane: The treated porous nanofiber composite membrane was placed in a tubular furnace under the protection of protective gas and carbonized at a temperature of 500 ℃~800 ℃ for 4 h at a heating rate of 5 ℃ / min to obtain a porous carbon nanofiber composite membrane.
[0010] Furthermore, in step (1), the method for preparing organic-metal organic framework (ZIF-67) powder is:
[0011] S1: Weigh cobalt nitrate hexahydrate (Co(NO3)2.6H2O) and 2-methylimidazole in a molar ratio of 1:3 and dissolve them in methanol respectively, then add the 2-methylimidazole solution to the cobalt nitrate hexahydrate, stir the mixed solution thoroughly, and let it stand for 24 hours;
[0012] S2: The mixed solution after standing was centrifuged at 8000 rpm for 10 min, and then washed with methanol for 4 to 5 times; then, vacuum dried for 12 h to obtain a powdered ZIF-67 product.
[0013] Preferably, in step (2), the dissolved cellulose and chitosan are mixed in a mass ratio of 3:7 to form a mixed spinning solution.
[0014] Furthermore, in step (2), cellulose and chitosan are dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid to form a spinning solution.
[0015] Furthermore, in step (2), when the high-voltage electrospinning device is spinning, the receiving distance of the device is 18 cm, the positive voltage is 16 kV, and the negative voltage is -2 kV.
[0016] Furthermore, in step (2), the nanofiber composite membrane is cleaned and dried by soaking the nanofiber composite membrane in 70% ethanol for 2 hours, filtering the nanofiber composite membrane several times, and drying the filtered fiber membrane in a vacuum drying oven at 60° C. for 4 hours.
[0017] Furthermore, in step (3), the protective gas includes nitrogen.
[0018] As an embodiment, the present invention provides a sodium ion battery negative electrode material, which is obtained by drying the porous carbon nanocomposite fiber membrane obtained by any of the preparation methods.
[0019] As another embodiment, the present invention provides a sodium ion battery, wherein the negative electrode material used in the sodium ion battery is the sodium ion battery negative electrode material obtained by the above-mentioned preparation method.
[0020] Compared with the prior art, the advantages of the present invention are:
[0021] In the present invention, two natural polymers with the most abundant reserves in nature, cellulose and chitosan, are used as raw materials, and a cobalt-based metal organic framework ZIF-67 with a large specific surface area, controllable pore structure, high conductivity, and uniformly dense active sites is introduced. Cellulose, chitosan, and ZIF-67 are compounded by high-voltage electrospinning to obtain porous composite nanofiber membranes with different structures, and the nanofiber composite membranes are carbonized to obtain the negative electrode material of the biomass / MOF composite sodium ion battery. This composite membrane can effectively improve the electrochemical performance and cycle stability of sodium ion batteries. The method has broad application prospects and can be widely used in the field of energy storage and conversion. It provides a new way to improve the performance of sodium ion batteries and makes an important contribution to the realization of efficient and sustainable energy storage solutions. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a morphology diagram of the cellulose, chitosan electrospinning combined with ZIF-67 nanofiber composite membrane grown in situ;
[0023] Figure 2 This is a morphology diagram of the nanofiber composite membrane of the present invention after carbonization by in-situ growth.
[0024] Figure 3 This is a morphology diagram of the cellulose and chitosan electrospinning combined with ZIF-67 nanofiber composite membrane by blending;
[0025] Figure 4 This is a morphology diagram of the nanofiber composite membrane of the present invention after carbonization by blending. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific examples, but these examples are only exemplary and do not constitute any limitation to the scope of the present invention. The molecular weight range of the cellulose used in the present invention is 2000-3000 g mol -1 , chitosan molecular weight is 1000-1500 g mol -1, the deacetylation degree is 90%~95%. All other reagents are analytically pure, all materials can be purchased from the market, and the high-voltage electrospinning device used (specification model ET-2535H) is used. Embodiment 1:
[0027] (1) Preparation of organic-metal organic framework (ZIF-67) powder
[0028] Weigh cobalt nitrate hexahydrate (Co(NO3)2.6H2O) and 2-methylimidazole (2-Hmim, 99%) in a molar ratio of 1:3 and dissolve them in methanol. Then add the 2-methylimidazole solution to the cobalt nitrate hexahydrate, stir and mix thoroughly, and let it stand for 24 hours. The mixture after standing was centrifuged at 8000rpm for 10 minutes, and then washed with methanol for 4 to 5 times. Finally, vacuum dry for 12 hours to obtain the purple powder ZIF-67 product.
[0029] (2) Preparation of biomass porous nanofiber composite membrane
[0030] Cellulose was dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid (EMM), and stirred in an oil bath for 6 hours to prepare 8wt% cellulose spinning solution; chitosan powder was dissolved in EMM, and stirred for 8 hours to prepare 6wt% chitosan spinning solution, and then the dissolved cellulose and chitosan were taken in a mass ratio of 3:7, and stirred evenly to form a mixed solution, ZIF-67 powder was added to the mixed solution, and the concentration of ZIF-67 was prepared to be 2wt%, and stirred evenly to obtain the spinning solution.
[0031] The spinning solution was spun using a high-voltage electrospinning device, with a receiving distance of 18 cm, a positive voltage of 16 kV, and a negative voltage of -2 kV to obtain a porous, ultra-soft nanofiber composite membrane. The collected nanofiber composite membrane was soaked in 70% ethanol for 2 hours, and then filtered several times. The filtered nanofiber composite membrane was placed in a vacuum drying oven at 60 ° C for 4 hours to obtain a porous nanofiber composite membrane.
[0032] (3) Preparation of biomass porous carbon nanofiber composite membrane
[0033] The treated porous nanofiber composite membrane was placed in a tubular furnace under nitrogen protection at a heating rate of 5°C / min and carbonized at 700°C for 4 h to obtain a porous carbon nanofiber composite membrane.
[0034] (4) Final product - sodium ion battery negative electrode material
[0035] The porous carbon nanocomposite fiber membrane was dried at 60°C for 2h in a vacuum drying oven, and then cut into discs with a diameter of 10mm as the negative electrode material C1. The negative electrode material C1 and metal sodium were combined into a button cell for electrochemical performance testing. Embodiment 2:
[0036] (1) Preparation of organic-metal organic framework (ZIF-67) powder
[0037] Weigh cobalt nitrate hexahydrate (Co(NO3)2.6H2O) and 2-methylimidazole (2-Hmim, 99%) in a molar ratio of 1:3 and dissolve them in methanol. Then add the 2-methylimidazole solution to the cobalt nitrate hexahydrate, stir and mix thoroughly, and let it stand for 24 hours. The mixed solution after standing was centrifuged at 8000rpm for 10 minutes, and then washed with methanol for 4 to 5 times. Finally, vacuum dried for 12 hours to obtain the purple powder ZIF-67 product.
[0038] (2) Preparation of biomass porous nanofiber composite membrane
[0039] Cellulose was dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid (EMM), and stirred in an oil bath for 6 hours to prepare 8wt% cellulose spinning solution; chitosan powder was dissolved in EMM, and stirred for 8 hours to prepare 6wt% chitosan spinning solution, and then the dissolved cellulose and chitosan were taken in a mass ratio of 2:8, and stirred evenly to form a mixed solution, ZIF-67 powder was added to the mixed solution, and the concentration of ZIF-67 was prepared to be 4wt%, and stirred evenly to obtain the spinning solution.
[0040] The spinning solution was spun using a high-voltage electrospinning device, with a receiving distance of 18 cm, a positive voltage of 16 kV, and a negative voltage of -2 kV to obtain a porous, ultra-soft nanofiber composite membrane. The collected nanofiber composite membrane was soaked in 70% ethanol for 2 hours, and then filtered several times. The filtered nanofiber composite membrane was placed in a vacuum drying oven at 60 ° C for 4 hours to obtain a porous nanofiber composite membrane.
[0041] (3) Preparation of biomass porous carbon nanofiber composite membrane
[0042] The treated porous nanofiber composite membrane was placed in a tubular furnace under nitrogen protection at a heating rate of 5°C / min and carbonized at 500°C for 4 h to obtain a porous carbon nanofiber composite membrane.
[0043] (4) Final product - sodium ion battery negative electrode material
[0044] The porous carbon nanocomposite fiber membrane was dried in a vacuum drying oven at 60° C. for 2 h, and then taken out and cut into discs with a diameter of 10 mm as negative electrode materials. Embodiment 3:
[0045] (1) Preparation of organic-metal organic framework (ZIF-67) powder
[0046] Weigh cobalt nitrate hexahydrate (Co(NO3)2.6H2O) and 2-methylimidazole (2-Hmim, 99%) in a molar ratio of 1:3 and dissolve them in methanol. Then add the 2-methylimidazole solution to the cobalt nitrate hexahydrate, stir and mix thoroughly, and let it stand for 24 hours. The mixed solution after standing was centrifuged at 8000rpm for 10 minutes, and then washed with methanol for 4 to 5 times. Finally, vacuum dried for 12 hours to obtain the purple powder ZIF-67 product.
[0047] (2) Preparation of biomass porous nanofiber composite membrane
[0048] Cellulose was dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid (EMM), and stirred in an oil bath for 6 hours to prepare 8wt% cellulose spinning solution; chitosan powder was dissolved in EMM, and stirred for 8 hours to prepare 6wt% chitosan spinning solution, and then the dissolved cellulose and chitosan were taken in a mass ratio of 8:2, and stirred evenly to form a mixed solution, ZIF-67 powder was added to the mixed solution, and the concentration of ZIF-67 was prepared to be 3wt%, and stirred evenly to obtain the spinning solution.
[0049] The spinning solution was spun using a high-voltage electrospinning device, with a receiving distance of 18 cm, a positive voltage of 16 kV, and a negative voltage of -2 kV to obtain a porous, ultra-soft nanofiber composite membrane. The collected nanofiber composite membrane was soaked in 70% ethanol for 2 hours, and then filtered several times. The filtered nanofiber composite membrane was placed in a vacuum drying oven at 60 ° C for 4 hours to obtain a porous nanofiber composite membrane.
[0050] (3) Preparation of biomass porous carbon nanofiber composite membrane
[0051] The treated porous nanofiber composite membrane was placed in a tubular furnace under nitrogen protection at a heating rate of 5°C / min and carbonized at 800°C for 4 h to obtain a porous carbon nanofiber composite membrane. Figure 2 shown.
[0052] (4) Final product - sodium ion battery negative electrode material
[0053] The porous carbon nanocomposite fiber membrane was dried in a vacuum drying oven at 60° C. for 2 h, and then taken out and cut into discs with a diameter of 10 mm as negative electrode materials.
[0054] Comparative Example 1
[0055] (1) Preparation of electrospinning solution
[0056] Cellulose was dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid (EMM), and stirred in an oil bath for 6 hours to prepare 8wt% cellulose spinning solution; chitosan powder was dissolved in EMM, and stirred for 8 hours to prepare 6wt% chitosan spinning solution. Then, the dissolved cellulose and chitosan were taken at a mass ratio of 3:7 and stirred evenly to obtain a mixed spinning solution.
[0057] (2) Preparation of cellulose / chitosan porous nanofiber membrane
[0058] The cellulose and chitosan mixed spinning solution was spun using a high-voltage electrospinning device, with a receiving distance of 18 cm, a positive voltage of 16 kV, and a negative voltage of -2 kV to obtain a porous, ultra-soft nanofiber membrane. The collected fiber membrane was soaked in ethanol for 2 hours, then filtered several times, and the filtered fiber membrane was placed in a vacuum drying oven at 60°C for 4 hours.
[0059] (3) Preparation of organic-metal organic framework (ZIF-67) solution
[0060] Cobalt nitrate hexahydrate (Co(NO3)2.6H2O) and 2-methylimidazole (2-Hmim, 99%) were weighed in a molar ratio of 1:3 and dissolved in methanol respectively. The 2-methylimidazole solution was then added to the cobalt nitrate hexahydrate, and the mixture was stirred thoroughly to obtain a ZIF-67 solution, which was then set aside for later use.
[0061] (4) Preparation of biomass porous nanofiber composite membrane
[0062] The nanofiber membrane prepared in (2) was cut into a square shape and placed in a culture dish. 15 mL of ZIF-67 solution was added and allowed to stand for 24 h to allow ZIF-67 to grow in situ on the nanofiber membrane. After standing for 12 h, the nanofiber composite membrane was ultrasonically washed 2 to 3 times with methanol solution and then vacuum dried at 60 °C for 2 h.
[0063] (5) Preparation of biomass porous carbon nanofiber composite membrane
[0064] The treated porous nanofiber membrane was placed in a tubular furnace under nitrogen protection at a heating rate of 5°C / min and carbonized at 700°C for 4 hours to obtain a porous carbon nanocomposite fiber membrane.
[0065] (6) Final product - sodium ion battery negative electrode material
[0066] The porous carbon nanocomposite fiber membrane was dried at 60°C for 2h in a vacuum drying oven, and then cut into discs with a diameter of 10mm as the negative electrode material C2. The negative electrode material C2 and metal sodium were combined into a button cell for electrochemical performance testing.
[0067] Comparative Example 2
[0068] (1) Preparation of electrospinning solution
[0069] Cellulose was dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid (EMM), and stirred in an oil bath for 6 hours to prepare 8wt% cellulose spinning solution; chitosan powder was dissolved in EMM, and stirred for 8 hours to prepare 6wt% chitosan spinning solution. The dissolved cellulose and chitosan were then mixed evenly at a mass ratio of 3:7 to obtain a mixed spinning solution.
[0070] (2) Preparation of cellulose / chitosan porous nanofiber membrane
[0071] The cellulose and chitosan mixed spinning solution was spun using a high-voltage electrospinning device, with a receiving distance of 18 cm, a positive voltage of 16 kV, and a negative voltage of -2 kV to obtain a porous, ultra-soft nanofiber membrane. The collected fiber membrane was soaked in 70% ethanol for 2 hours, then filtered several times, and the filtered fiber membrane was placed in a vacuum drying oven at 60 ° C for 4 hours.
[0072] (3) Preparation of biomass porous carbon nanofiber composite membrane
[0073] The treated porous nanofiber membrane was placed in a tubular furnace under nitrogen protection at a heating rate of 5°C / min and carbonized at 700°C for 4 h to obtain a porous carbon nanocomposite fiber membrane.
[0074] (4) Final product - sodium ion battery negative electrode material
[0075] The porous carbon nanocomposite fiber membrane was dried at 60°C for 2h in a vacuum drying oven, and then cut into discs with a diameter of 10mm as the negative electrode material C3. The negative electrode material C3 and metal sodium were combined into a button cell for electrochemical performance testing.
[0076] Comparative Example 3
[0077] (1) Preparation of biomass composite membrane
[0078] Cellulose was dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid (EMM), and stirred in an oil bath for 6 hours to prepare 8wt% cellulose spinning solution; chitosan powder was dissolved in EMM, and stirred for 8 hours to prepare 6wt% chitosan spinning solution. Then, the dissolved cellulose and chitosan were mixed evenly at a mass ratio of 3:7 to form a spinning mixture.
[0079] The cellulose / chitosan composite membrane was obtained by spin coating. The collected fiber membrane was soaked in 70% ethanol for 2 h, then filtered several times, and the filtered fiber membrane was placed in a vacuum drying oven at 60°C for 4 h.
[0080] (2) Preparation of biomass porous carbon nanofiber composite membrane
[0081] The treated cellulose / chitosan composite membrane was placed in a tubular furnace under nitrogen protection at a heating rate of 5°C / min and carbonized at 700°C for 4 h to obtain a composite carbon membrane.
[0082] (3) Final product - sodium ion battery negative electrode material
[0083] The composite carbon film was dried at 60°C in a vacuum oven for 2 h, and then cut into discs with a diameter of 10 mm as the negative electrode material C4. The negative electrode material C4 and metal sodium were combined into a button cell for electrochemical performance testing.
[0084] Sodium button battery assembly method: First, prepare the materials. Use the prepared carbon nanofibers (C1, C2, C3, C4) as the negative electrode material, cut the metal sodium sheet into 10mm as the positive electrode material, use sodium hypochlorite as the electrolyte, prepare basic equipment such as gaskets, positive and negative electrode shells and diaphragms, and place the above materials in a vacuum glove box for standby use. Secondly, assemble the battery. Place the negative electrode shell at the bottom layer, and add the negative electrode material, electrolyte, diaphragm, electrolyte, positive electrode material, gasket, and positive electrode shell in turn. Finally, use a sealing machine to seal the assembled battery to obtain a complete sodium button battery.
[0085] Electrochemical performance test method: The button battery is mainly tested for cycle life and constant current charge and discharge performance using a blue electric test system. During the constant current charge and discharge test, the current density is 100 mA g -1 and 1000mA g -1 .
[0086] The comparison of electrochemical performance indicators of the nanobatteries obtained in the above examples is shown in Table 1 below:
[0087] Table 1 Performance indicators of each tested product
[0088]
[0089] It can be seen from the electrochemical performance of the sodium battery prepared in Table 1 that the negative electrode material prepared by the present invention has more excellent specific capacity, cycle stability and rate performance than the comparative example. In terms of the preparation method, Example 1 of the present invention and Comparative Example 1 adopt two different ways of introducing MOF particles.
[0090] In Example 1, MOF particles are first prepared, and then blended with cellulose and chitosan to form a composite fiber membrane; while in Comparative Example 1, cellulose and chitosan composite fibers are first prepared, and then MOF particles are in situ grown and loaded. Different preparation steps lead to significant performance differences. The negative electrode material obtained under the preparation steps of Comparative Example 1 is as follows Figure 1 , 2As shown in the figure, ZIF-67 is evenly loaded on the surface of the fiber, and after pyrolysis, it presents a loose porous structure, which is conducive to conductivity. However, ZIF-67 prepared in this way is easy to fall off, and it cannot ensure that the surface of each fiber is evenly loaded with Co nanoparticles. Compared with pure cellulose and chitosan, the conductivity is further improved in terms of performance. The negative electrode material prepared in Example 1 is as follows Figure 3 , 4 As shown in the figure, it can be seen that the ZIF-67 wrapped in the fiber membrane shrinks due to pyrolysis, squeezing the formed Co nanoparticles to the surface of the fiber, and its structure is more stable. Compared with the in-situ growth method, the uniform conductive ions further improve the conductivity.
[0091] The main difference between Comparative Example 2 and Example 1 is whether the metal organic framework material (ZIF-67) is added. According to the data, the discharge specific capacity of Comparative Example 2 is much lower than that of Example 1. This result is because the use of pure biomass raw materials as negative electrode materials has a certain conductivity, but the conductivity is weak. The Co nanoparticles contained in ZIF-67 can effectively participate in the conductive process, thereby improving the overall conductive performance.
[0092] Comparative Example 3 is a horizontal comparison with Comparative Example 2, which mainly compares the effects of different preparation methods on the electrochemical properties of nanofiber membranes. Comparative Example 3 uses a spin coating method, while Comparative Example 2 uses an electrostatic spinning method. According to the data, it can be found that the conductivity of the nanofiber membrane prepared by the spin coating method is generally lower than that of the electrostatic spinning method. The reason for this result is that the spin coating method is to apply the solution by rotating the substrate, so the arrangement of the nanofibers may not be uniform enough, and there are problems such as fiber crossing and stacking, while the fibers prepared by electrostatic spinning are usually arranged more uniformly. Therefore, this comparative example is not only compared from the addition or not of the metal organic framework material, but also from different preparation methods. This further highlights that the present invention uses electrostatic spinning technology to prepare the biomass-metal organic framework negative electrode material, which provides excellent conductivity for sodium ion batteries.
[0093] In summary, the raw materials of the present invention are abundant in source and green and renewable. By adopting electrospinning technology, a high specific surface area and porous structure can be provided for the biomass-based negative electrode material, which is conducive to the electrochemical reaction and the movement of conductive ions. The nanofiber membrane is combined with metal-organic frameworks (MOFs) to further increase the specific surface area and conductivity of the electrode material, and the introduction of a special structure of the metal-organic framework can promote the sodium ion (Na +) movement, improving the electrochemical properties of the material, overcoming the limited conductivity and specific surface area of traditional hard carbon materials, and low theoretical capacity. The composite method effectively solves the shortcomings of MOF materials such as high brittleness, easy agglomeration, poor processability and difficult molding. The prepared ultra-soft and porous carbon nanofiber composite membrane has excellent specific capacity, cycle stability and rate performance when used as a negative electrode material.
[0094] The above description is merely a further detailed explanation of the present invention, but not a limitation of the present invention. A person skilled in the art in the field to which the present invention belongs may make several derivations, modifications or substitutions without departing from the concept of the present invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application and are protected by the patent law.
Claims
1. A method for preparing a biomass / metal-organic framework (MOFs) sodium ion battery negative electrode material, characterized in that: The following steps are involved: (1) Preparation of ZIF-67 powder; (2) Preparing a biomass porous nanofiber composite membrane: preparing an 8 wt% cellulose spinning solution; preparing a 6 wt% chitosan spinning solution, and then mixing the dissolved cellulose and chitosan in a mass ratio of 2:8 to 8:2 to form a mixed solution, adding ZIF-67 powder to the mixed solution to prepare a concentration of 2 to 4 wt% ZIF-67, stirring evenly to obtain a spinning solution, spinning using a high-voltage electrospinning device to obtain a nanofiber composite membrane, and washing and drying the nanofiber composite membrane for later use; (3) Preparation of biomass porous carbon nanofiber composite membrane: The treated porous nanofiber composite membrane is placed in a tubular furnace under the protection of a protective gas and carbonized at a temperature of 500°C to 800°C for 4 h at a heating rate of 5°C / min to obtain a porous carbon nanofiber composite membrane, wherein the protective gas is nitrogen.
2. The preparation method according to claim 1, characterized in that: In step (1), the method for preparing organic-metal organic framework (ZIF-67) powder is: S1: Weigh cobalt nitrate hexahydrate (Co(NO3)2.6H2O) and 2-methylimidazole in a molar ratio of 1:3 and dissolve them in methanol respectively, then add the 2-methylimidazole solution to the cobalt nitrate hexahydrate, stir the mixed solution thoroughly, and let it stand for 24 hours; S2: The mixed solution after standing was centrifuged at 8000 rpm for 10 min, and then washed with methanol for 4 to 5 times; then, vacuum dried for 12 h to obtain a powdered ZIF-67 product.
3. The preparation method according to claim 1, characterized in that: In step (2), the dissolved cellulose and chitosan are mixed in a mass ratio of 3:7 to form a mixed solution.
4. The preparation method according to claim 1, characterized in that: In step (2), cellulose and chitosan are dissolved in 1-ethyl-3-methylimidazolium acetate ionic liquid.
5. The preparation method according to claim 1, characterized in that: In step (2), when the high-voltage electrospinning device is spinning, the receiving distance of the device is 18 cm, the positive voltage is 16 kV, and the negative voltage is -2 kV.
6. The preparation method according to claim 1, characterized in that: In step (2), the nanofiber composite membrane is cleaned and dried by soaking the nanofiber composite membrane in 70% ethanol for 2 hours, filtering the nanofiber composite membrane several times, and drying the filtered fiber membrane in a vacuum drying oven at 60° C. for 4 hours.
7. A sodium ion battery negative electrode material, characterized in that: The porous carbon nanocomposite fiber membrane obtained by any preparation method according to any one of claims 1 to 6 is dried to obtain the battery negative electrode material.
8. A sodium ion battery, characterized in that: The negative electrode material of the sodium ion battery is the negative electrode material of the sodium ion battery according to claim 7.