A stem cell composition for promoting skin wound healing and preparation method thereof

By preparing a combination of carrier and biological antibacterial agent, and using cross-linked chitosan gel particles and cyclodextrin metal-organic framework materials, the problem of poor antibacterial properties and thickening of stem cell growth factor for external use on the skin has been solved, and the treatment of Effective healing and antibacterial effects on scabbed wounds, and easy to use.

CN118236399BActive Publication Date: 2024-10-01SHANDONG KANGYUAN BIOLOGICAL GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410649674.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-10-01
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

Existing stem cell growth factor skin drugs have poor antibacterial properties, may aggravate skin infections, cause skin hyperplasia and thickening, have poor healing effects on scabbed wounds, and are complex and difficult to use.

Method used

A method for preparing a stem cell composition is adopted, by preparing a carrier and a biological antibacterial agent, using cross-linked chitosan gel particles to composite with calcium phosphate, and combining cyclodextrin metal-organic framework materials and small molecular weight zinc hyaluronate to form Compositions with antibacterial and sustained-release effects for promoting skin wound healing.

Benefits of technology

The composition can accelerate wound healing, promote regeneration of scabbed wounds, has good antibacterial properties, avoids skin proliferation and thickening, is easy to use, and is suitable for direct application to wounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

A stem cell composition for promoting skin wound healing and a preparation method thereof belong to the technical field of skin wound repair, and are composed of the following steps: preparing a carrier, preparing a biological antibacterial agent, culturing stem cells, and combining; the preparation of the carrier is composed of the following steps: preparing gel particles and compounding; the preparation of the biological antibacterial agent is composed of the following steps: preparing a metal-organic framework material, preparing an inclusion compound, and mixing; the stem cell composition of the invention can accelerate wound healing and promote skin regeneration at a scabbed wound, has good antibacterial property, will not cause skin hyperplasia and thickening, and is easy to use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of skin wound repair, and in particular to a stem cell composition for promoting skin wound healing and a preparation method thereof. Background Art

[0002] Stem cells are a type of cell that has unlimited or immortal self-renewal capabilities and can produce at least one type of highly differentiated daughter cells. The effects of stem cells on the skin are mainly reflected in care and repair. They can promote the regeneration of skin cells, repair damaged tissues, and delay skin aging. When repairing damaged tissues, stem cells can secrete a variety of growth factors that help repair damaged skin tissues. For example, for skin injuries such as burns and scars, stem cells can accelerate wound healing and reduce scar formation by secreting growth factors and cytokines. Therefore, stem cell growth factors are widely used in topical skin medications.

[0003] However, the skin topical medications prepared from stem cell growth factors have the following problems during use: stem cell growth factors do not have antibacterial properties. For skin wounds that have already been infected, it is not only difficult for stem cell growth factors to accelerate wound healing, but they may also aggravate skin infections; after acting on the wounds, stem cell growth factors can stimulate skin cells to multiply rapidly, causing the skin to proliferate, thicken, harden, and become rough, and skin nodules may also appear; for wounds that have not scabbed, they can accelerate the healing of scabs, but for wounds that have already scabbed, due to the poor transdermal properties of stem cell growth factors, stem cell growth factors cannot penetrate the skin to stimulate skin regeneration, which further leads to poor effects of stem cell growth factors.

[0004] To address the above problems, the most commonly used solutions are: by adding stem cell growth factors and antibacterial drugs, such as antibiotics, imidazole antibiotics, and acrylamine antibiotics, to topical skin medications at the same time, thereby improving the antibacterial properties of topical skin medications; by controlling the dosage and frequency of topical skin medications, reducing the stimulating effects of stem cell growth factors and avoiding skin hyperplasia, thickening, hardening, and roughening; by using injections or microneedle introduction methods, allowing stem cell growth factors to penetrate the skin, thereby stimulating skin regeneration.

[0005] However, the above-mentioned solutions have the following problems: antimicrobial drugs inhibit the activity of stem cell growth factor, which will lead to a decrease in the effect of stem cell growth factor; by controlling the dosage and frequency of use, the problem of skin hyperplasia and thickening caused by stem cell growth factor can only be alleviated to a certain extent, and the problem cannot be solved fundamentally; injection or microneedle introduction will lead to a high concentration of growth factor at the injection or microneedle introduction site, promoting rapid reproduction of skin cells at this site, aggravating the problem of skin hyperplasia and thickening; and compared with direct application to the skin, the operation of injection or microneedle introduction is complicated, resulting in high difficulty in using stem cell growth factor.

[0006] Therefore, the development of a stem cell composition that promotes skin wound healing can accelerate wound healing while promoting skin regeneration at scabby wounds, has good antibacterial properties, does not cause skin hyperplasia and thickening, and is easy to use, which is of great technical significance. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention provides a stem cell composition for promoting skin wound healing and a preparation method thereof, which can accelerate wound healing while promoting skin regeneration at scabby wounds, has good antibacterial properties, will not cause skin hyperplasia and thickening, and is easy to use.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0009] A method for preparing a stem cell composition for promoting skin wound healing, comprising the following steps: preparing a carrier, preparing a biological antibacterial agent, culturing stem cells, and combining;

[0010] The preparation of the carrier comprises the following steps: preparing gel particles, compounding;

[0011] The gel particles are prepared by dissolving chitosan in an acetic acid aqueous solution, stirring at a stirring speed of 300-500 rpm for 10-15 minutes at room temperature, adding a genipin aqueous solution, stirring at a stirring speed of 300-500 rpm for 5-10 minutes at room temperature to obtain a dispersed phase; adding Span 80 to liquid paraffin, stirring at a stirring speed of 300-500 rpm for 15-20 minutes at room temperature, adding all the above dispersed phases, shearing at a shearing speed of 10000-12000 rpm for 3-5 minutes at room temperature, stirring at a stirring speed of 300-500 rpm for 9-10 hours at room temperature, adding anhydrous ethanol, continuing to stir at a stirring speed of 300-500 rpm for 50-60 minutes at room temperature, centrifuging at a speed of 6000-7000 rpm for 5-6 minutes, washing the precipitate 4-5 times with anhydrous ethanol of 20-30 times the volume of the precipitate, and vacuum drying at 70-80° C. to constant weight to obtain gel particles;

[0012] In the preparation of the gel particles, the mass volume ratio of chitosan, acetic acid aqueous solution, genipin aqueous solution, Span 80, liquid paraffin, and anhydrous ethanol is 1.8-2g:100-120mL:11-13mL:23-25mL:550-600mL:600-700mL;

[0013] The mass concentration of the acetic acid aqueous solution is 1.4-1.6%;

[0014] The mass concentration of the genipin aqueous solution is 0.5-0.6%;

[0015] The number average molecular weight of the chitosan is 100 kDa, and the degree of deacetylation is 95%;

[0016] The composite comprises mixing the gel particles and deionized water, stirring at a stirring speed of 300-500 rpm for 30-50 minutes at room temperature, adding a calcium chloride aqueous solution, continuing stirring for 40-60 minutes, adjusting the pH to 9.5-10, dripping an ammonium phosphate aqueous solution, and adjusting the pH to 9.5-10 during the dripping process. After the dripping is completed, centrifuging at a speed of 5000-6000 rpm for 5-6 minutes, washing the precipitate 4-5 times with deionized water of 20-30 times the volume of the precipitate, and vacuum drying at 70-80° C. to constant weight to obtain a carrier;

[0017] The composite, gel particles, deionized water, calcium chloride aqueous solution, ammonium phosphate aqueous solution mass volume ratio is 20-25g:300-350mL:130-150mL:50-60mL;

[0018] The mass concentration of the calcium chloride aqueous solution is 5%;

[0019] The mass concentration of the ammonium phosphate aqueous solution is 4%;

[0020] The dropping speed of the ammonium phosphate aqueous solution is 4-5 mL / min;

[0021] The preparation of the biological antibacterial agent comprises the following steps: preparing a metal-organic framework material, preparing an inclusion compound, and mixing;

[0022] The metal-organic framework material is prepared by mixing zinc chloride, β-cyclodextrin and deionized water, stirring at room temperature at a stirring speed of 300-500 rpm for 10-15 minutes, adding anhydrous ethanol, continuing stirring for 50-60 minutes, performing a hydrothermal reaction at 70-90° C. for 18-20 hours, filtering, washing the filter residue with anhydrous ethanol 20-30 times the volume of the filter residue for 3-5 times, and vacuum drying at 70-80° C. to constant weight to obtain the metal-organic framework material;

[0023] In the preparation of the metal-organic framework material, the mass volume ratio of zinc chloride, β-cyclodextrin, deionized water, and anhydrous ethanol is 2.8-3 g:11-13 g:1000-1200 mL:3.5-4 mL;

[0024] The inclusion compound is prepared by mixing the metal-organic framework material and deionized water, stirring at a stirring speed of 300-500 rpm for 20-30 minutes at room temperature, adding fat-soluble vitamin E, ultrasonically oscillating at a frequency of 20-25 kHz for 50-60 minutes at room temperature, standing at room temperature for 10-12 hours, filtering, and vacuum drying the filter residue at 50-60° C. to constant weight to obtain the inclusion compound;

[0025] In the preparation of the inclusion compound, the mass volume ratio of the metal-organic framework material, deionized water, and fat-soluble vitamin E is 3.5-3.7 g:100-105 mL:6.5-7.5 g;

[0026] The mixing comprises mixing the gel particles prepared in the step of preparing the gel particles in the step of preparing the carrier, the inclusion compound, the low molecular weight hyaluronate zinc, and deionized water, stirring at room temperature at a stirring speed of 300-500 rpm for 1-1.5 hours, filtering, and vacuum drying the filter residue at 70-80° C. to constant weight to obtain a biological antibacterial agent;

[0027] In the mixing, the mass volume ratio of the gel particles prepared in the step of preparing the gel particles in the step of preparing the carrier, the inclusion compound, the low molecular weight hyaluronate zinc, and the deionized water is 200-210g:70-80g:20-25g:3000-3500mL;

[0028] The number average molecular weight of the low molecular weight zinc hyaluronate is 10 kDa;

[0029] The stem cells are cultured by selecting active human placental mesenchymal stem cells from a cell bank, culturing them in a phenol red-free DMEM medium at a temperature of 37-39° C. and a carbon dioxide volume concentration of 5-6% to a growth density of 75-80%, washing the cells 3-4 times with a PBS buffer, culturing them in a phenol red-free DMEM medium at a temperature of 37-39° C. and a carbon dioxide volume concentration of 5-6% to a growth density of 90-95%, centrifuging the supernatant in the culture medium to obtain a supernatant containing exosomes, filtering the supernatant containing exosomes using a filter membrane with a pore size of 0.22 μm, and obtaining the filtrate as exosomes.

[0030] The combination comprises mixing exosomes, a carrier and deionized water, stirring at a stirring speed of 300-500 rpm for 15-20 min at room temperature, adding xanthan gum, a biological antibacterial agent, sodium hyaluronate, sodium carboxymethyl cellulose and polyvinyl alcohol 1788, and continuing to stir for 1.5-2 h to obtain a stem cell composition;

[0031] In the combination, the mass volume ratio of exosomes, carrier, deionized water, xanthan gum, biological antibacterial agent, sodium hyaluronate, sodium carboxymethyl cellulose, and polyvinyl alcohol 1788 is 450-500 mL: 13-14 g: 240-260 mL: 8-10 g: 6-7 g: 3-4 g: 2-3 g: 1-2 g;

[0032] The molecular weight of the sodium hyaluronate is 1000 kDa.

[0033] A stem cell composition for promoting skin wound healing prepared by the aforementioned preparation method.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) The preparation method of the stem cell composition for promoting skin wound healing of the present invention comprises the following steps: in preparing a carrier, cross-linked chitosan gel particles are compounded with calcium phosphate, and calcium phosphate is loaded on the pores and surface of the cross-linked chitosan gel particles, thereby increasing the adsorption area and adsorption capacity, thereby increasing the adsorption amount, and reducing the pore size, thereby improving the sustained release effect. In addition, the use of cross-linked chitosan gel particles in the carrier can also utilize the antibacterial effect of chitosan to make the prepared stem cell composition have antibacterial ability; in preparing a biological antibacterial agent, a cyclodextrin metal-organic framework material is first prepared, and then the cavity of cyclodextrin in the cyclodextrin metal-organic framework material is used to encapsulate fat-soluble vitamin E, thereby slowing down the release of fat-soluble vitamin E. Release, during the mixing, the inclusion cyclodextrin metal-organic framework material and low molecular weight hyaluronate zinc are bonded to the surface of the gel particles, which can promote the dispersion and prevent the loss of the cyclodextrin metal-organic framework material, and can play a role in sustained release of the low molecular weight hyaluronate zinc. In the process of sustained release of the growth factor by the carrier, vitamin E can also be sustained released. Both vitamin E and low molecular weight hyaluronate zinc have excellent transdermal properties and can drive the skin to absorb the growth factor. The zinc ions in the low molecular weight hyaluronate zinc can further improve the skin's absorption capacity of the growth factor. In addition, due to the good bactericidal property of zinc ions, the antibacterial ability of the prepared stem cell composition can be further improved;

[0036] (2) The stem cell composition for promoting skin wound healing of the present invention can accelerate wound healing. In a test conducted on male SD rats, fascia injuries were completely healed after 10 days of use when the stem cell composition of the present invention was used daily after the injury.

[0037] (3) The stem cell composition for promoting skin wound healing of the present invention can promote skin regeneration in scab-formed wounds. In a test conducted on male SD rats, the fascia damage after scab formation was restored to normal skin after 10 days of use by using the stem cell composition of the present invention daily.

[0038] (4) The stem cell composition of the present invention for promoting skin wound healing has good antibacterial properties. In a test conducted on male SD rats, fascia injuries were infected with Staphylococcus aureus solution. The treatment was continued for 2 days after the onset of infection, and then the stem cell composition of the present invention was used daily. After 15 days of use, the wound was completely healed without infection.

[0039] (5) The stem cell composition for promoting skin wound healing of the present invention does not cause skin hyperplasia and thickening. In a test conducted on male SD rats, no skin hyperplasia and thickening occurred after daily use of the stem cell composition of the present invention for fascia injury.

[0040] (6) The stem cell composition for promoting skin wound healing of the present invention can be directly applied to the wound when used, and is convenient to use. DETAILED DESCRIPTION

[0041] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.

[0042] Example 1

[0043] A method for preparing a stem cell composition for promoting skin wound healing, specifically comprising:

[0044] 1. Preparation of carrier:

[0045] (1) Preparation of gel particles: 1.8 g of chitosan was dissolved in 100 mL of 1.4% acetic acid aqueous solution, stirred at 300 rpm for 10 min at room temperature, 11 mL of 0.5% genipin aqueous solution was added, and stirred at 300 rpm for 5 min at room temperature to obtain a dispersed phase; 23 mL of Span 80 was added to 550 mL of liquid paraffin, and stirred at 300 rpm for 15 min at room temperature, all of the above dispersed phases were added, sheared at 10,000 rpm for 3 min at room temperature, stirred at 300 rpm for 9 h at room temperature, 600 mL of anhydrous ethanol was added, and continued to stir at 300 rpm for 50 min at room temperature, centrifuged at 6,000 rpm for 5 min, and the precipitate was washed 4 times with 20 times the volume of anhydrous ethanol, and vacuum dried at 70°C to constant weight to obtain gel particles;

[0046] The number average molecular weight of the chitosan is 100 kDa, and the degree of deacetylation is 95%;

[0047] (2) Compounding: 20 g of gel particles and 300 mL of deionized water were mixed, and stirred at 300 rpm for 30 min at room temperature. 130 mL of 5% calcium chloride aqueous solution was added, and stirring was continued for 40 min. The pH was adjusted to 9.5, and 50 mL of 4% ammonium phosphate aqueous solution was added dropwise at a rate of 4 mL / min. The pH was always adjusted to 9.5 during the addition process. After the addition was completed, the mixture was centrifuged at 5000 rpm for 5 min. The precipitate was washed four times with deionized water 20 times the volume of the precipitate, and vacuum dried at 70°C to constant weight to obtain a carrier.

[0048] 2. Preparation of biological antibacterial agents:

[0049] (1) Preparation of metal-organic framework materials: 2.8 g zinc chloride, 11 g β-cyclodextrin, and 1000 mL deionized water were mixed, stirred at 300 rpm for 10 min at room temperature, 3.5 mL anhydrous ethanol was added, and stirring was continued for 50 min. The mixture was subjected to hydrothermal reaction at 70 °C for 18 h, filtered, and the residue was washed three times with anhydrous ethanol 20 times the volume of the residue. The residue was vacuum dried at 70 °C to constant weight to obtain a metal-organic framework material.

[0050] (2) Preparation of inclusion complex: 3.5 g of metal-organic framework material and 100 mL of deionized water were mixed, stirred at 300 rpm for 20 min at room temperature, 6.5 g of fat-soluble vitamin E was added, ultrasonically oscillated at 20 kHz for 50 min at room temperature, allowed to stand at room temperature for 10 h, filtered, and the residue was vacuum dried at 50 °C to constant weight to obtain an inclusion complex;

[0051] (3) Mixing: 200 g of the gel particles prepared in step (1) of the carrier preparation in step 1, 70 g of the inclusion compound, 20 g of low molecular weight zinc hyaluronate, and 3000 mL of deionized water were mixed, and the mixture was stirred at room temperature at a stirring speed of 300 rpm for 1 h, filtered, and the filter residue was vacuum dried at 70° C. to constant weight to obtain a biological antibacterial agent;

[0052] The number average molecular weight of the low molecular weight zinc hyaluronate is 10 kDa;

[0053] 3. Cultivation of stem cells: Active human placental mesenchymal stem cells were selected from the cell bank, cultured in phenol red-free DMEM medium at a temperature of 37°C and a carbon dioxide volume concentration of 5% to a growth density of 75%, washed the cells 3 times with PBS buffer, cultured in phenol red-free DMEM medium at a temperature of 37°C and a carbon dioxide volume concentration of 5% to a growth density of 90%, centrifuged the supernatant in the culture medium to obtain a supernatant containing exosomes, filtered the supernatant containing exosomes using a filter membrane with a pore size of 0.22 μm, and the filtrate obtained was the exosomes.

[0054] 4. Combination: 450 mL of exosomes, 13 g of carrier, and 240 mL of deionized water were mixed, and stirred at 300 rpm for 15 min at room temperature, 8 g of xanthan gum, 6 g of biological antibacterial agent, 3 g of sodium hyaluronate, 2 g of sodium carboxymethyl cellulose, and 1 g of polyvinyl alcohol 1788 were added, and the mixture was stirred for 1.5 h to obtain a stem cell composition;

[0055] The molecular weight of the sodium hyaluronate is 1000 kDa.

[0056] This embodiment also provides a stem cell composition for promoting skin wound healing prepared by the aforementioned preparation method.

[0057] Example 2

[0058] A method for preparing a stem cell composition for promoting skin wound healing, specifically comprising:

[0059] 1. Preparation of carrier:

[0060] (1) Preparation of gel particles: 1.9 g of chitosan was dissolved in 110 mL of 1.5% acetic acid aqueous solution, stirred at 400 rpm for 12 min at room temperature, 12 mL of 0.5% genipin aqueous solution was added, and stirred at 400 rpm for 8 min at room temperature to obtain a dispersed phase; 24 mL of Span 80 was added to 580 mL of liquid paraffin, and stirred at 400 rpm for 18 min at room temperature, all of the above dispersed phases were added, sheared at 11000 rpm for 4 min at room temperature, stirred at 400 rpm for 9.5 h at room temperature, 650 mL of anhydrous ethanol was added, and continued to stir at 400 rpm for 55 min at room temperature, centrifuged at 6500 rpm for 5 min, and the precipitate was washed 4 times with 25 times the volume of anhydrous ethanol, and vacuum dried at 75°C to constant weight to obtain gel particles;

[0061] The number average molecular weight of the chitosan is 100 kDa, and the degree of deacetylation is 95%;

[0062] (2) Compounding: 22 g of gel particles and 320 mL of deionized water were mixed, stirred at 400 rpm for 40 min at room temperature, 140 mL of 5% calcium chloride aqueous solution was added, stirring was continued for 50 min, the pH was adjusted to 9.5, 55 mL of 4% ammonium phosphate aqueous solution was added dropwise, the dropping speed was controlled to 4 mL / min, and the pH was always adjusted to 9.7 during the dropping process. After the dropping was completed, the mixture was centrifuged at 5500 rpm for 5 min, the precipitate was washed 4 times with 25 times the volume of the precipitate deionized water, and vacuum dried at 75°C to constant weight to obtain a carrier;

[0063] 2. Preparation of biological antibacterial agents:

[0064] (1) Preparation of metal-organic framework materials: 2.9 g zinc chloride, 12 g β-cyclodextrin, and 1100 mL deionized water were mixed, stirred at 400 rpm for 12 min at room temperature, 3.7 mL anhydrous ethanol was added, stirring was continued for 55 min, and hydrothermal reaction was carried out at 80 ° C for 19 h. The residue was filtered, and the residue was washed four times with anhydrous ethanol 25 times the volume of the residue, and vacuum dried at 75 ° C to constant weight to obtain a metal-organic framework material;

[0065] (2) Preparation of inclusion complex: 3.6 g of metal-organic framework material and 102 mL of deionized water were mixed, stirred at 400 rpm for 25 min at room temperature, 7 g of fat-soluble vitamin E was added, ultrasonically oscillated at 22 kHz for 55 min at room temperature, allowed to stand at room temperature for 11 h, filtered, and the residue was vacuum dried at 55 °C to constant weight to obtain an inclusion complex;

[0066] (3) Mixing: 205 g of the gel particles prepared in step (1) of the carrier preparation in step 1, 75 g of the inclusion compound, 22 g of low molecular weight zinc hyaluronate, and 3200 mL of deionized water were mixed, and the mixture was stirred at room temperature at a stirring speed of 400 rpm for 1.2 h, filtered, and the filter residue was vacuum dried at 75° C. to constant weight to obtain a biological antibacterial agent;

[0067] The number average molecular weight of the low molecular weight zinc hyaluronate is 10 kDa;

[0068] 3. Cultivation of stem cells: Active human placental mesenchymal stem cells were selected from the cell bank, cultured in phenol red-free DMEM medium at a temperature of 38°C and a carbon dioxide volume concentration of 5% to a growth density of 75%, washed the cells 3 times with PBS buffer, cultured in phenol red-free DMEM medium at a temperature of 38°C and a carbon dioxide volume concentration of 5% to a growth density of 90%, centrifuged the supernatant in the culture medium to obtain a supernatant containing exosomes, filtered the supernatant containing exosomes using a filter membrane with a pore size of 0.22 μm, and the filtrate obtained was the exosomes.

[0069] 4. Combination: 480 mL of exosomes, 13.5 g of carrier, and 250 mL of deionized water were mixed, and stirred at 400 rpm for 18 min at room temperature, and 9 g of xanthan gum, 6.5 g of biological antibacterial agent, 3.5 g of sodium hyaluronate, 2.5 g of sodium carboxymethyl cellulose, and 1.5 g of polyvinyl alcohol 1788 were added and mixed, and the mixture was stirred for 1.5 h to obtain a stem cell composition;

[0070] The molecular weight of the sodium hyaluronate is 1000 kDa.

[0071] This embodiment also provides a stem cell composition for promoting skin wound healing prepared by the aforementioned preparation method.

[0072] Example 3

[0073] A method for preparing a stem cell composition for promoting skin wound healing, specifically comprising:

[0074] 1. Preparation of carrier:

[0075] (1) Preparation of gel particles: 2 g of chitosan was dissolved in 120 mL of 1.6% acetic acid aqueous solution, stirred at 500 rpm for 15 min at room temperature, 13 mL of 0.6% genipin aqueous solution was added, and stirred at 500 rpm for 10 min at room temperature to obtain a dispersed phase; 25 mL of Span 80 was added to 600 mL of liquid paraffin, and stirred at 500 rpm for 20 min at room temperature, all of the above dispersed phases were added, sheared at 12000 rpm for 5 min at room temperature, stirred at 500 rpm for 10 h at room temperature, 700 mL of anhydrous ethanol was added, and continued to stir at 500 rpm for 60 min at room temperature, centrifuged at 7000 rpm for 6 min, and the precipitate was washed 5 times with anhydrous ethanol 30 times the volume of the precipitate, and vacuum dried at 80°C to constant weight to obtain gel particles;

[0076] The number average molecular weight of the chitosan is 100 kDa, and the degree of deacetylation is 95%;

[0077] (2) Compounding: 25 g of gel particles and 350 mL of deionized water were mixed, stirred at 500 rpm for 50 min at room temperature, 150 mL of 5% calcium chloride aqueous solution was added, stirring was continued for 60 min, the pH was adjusted to 10, 60 mL of 4% ammonium phosphate aqueous solution was added dropwise, the dropping speed was controlled to 5 mL / min, and the pH was always adjusted to 10 during the dropping process. After the dropping was completed, the mixture was centrifuged at 6000 rpm for 6 min, the precipitate was washed 5 times with 30 times the volume of deionized water, and vacuum dried at 80°C to constant weight to obtain a carrier;

[0078] 2. Preparation of biological antibacterial agents:

[0079] (1) Preparation of metal-organic framework materials: 3 g zinc chloride, 13 g β-cyclodextrin, and 1200 mL deionized water were mixed, stirred at room temperature at a stirring speed of 500 rpm for 15 min, 4 mL anhydrous ethanol was added, and stirring was continued for 60 min. The mixture was subjected to hydrothermal reaction at 90 °C for 20 h, filtered, and the residue was washed five times with anhydrous ethanol 30 times the volume of the residue. The residue was vacuum dried at 80 °C to constant weight to obtain a metal-organic framework material.

[0080] (2) Preparation of inclusion complex: 3.7 g of metal-organic framework material and 105 mL of deionized water were mixed, stirred at 500 rpm for 30 min at room temperature, 7.5 g of fat-soluble vitamin E was added, ultrasonically oscillated at 25 kHz for 60 min at room temperature, allowed to stand at room temperature for 12 h, filtered, and the residue was vacuum dried at 60 °C to constant weight to obtain an inclusion complex;

[0081] (3) Mixing: 210 g of the gel particles prepared in step (1) of the carrier preparation in step 1, 80 g of the inclusion compound, 25 g of low molecular weight zinc hyaluronate, and 3500 mL of deionized water were mixed, and the mixture was stirred at room temperature at a stirring speed of 500 rpm for 1.5 h, filtered, and the filter residue was vacuum dried at 80° C. to constant weight to obtain a biological antibacterial agent;

[0082] The number average molecular weight of the low molecular weight zinc hyaluronate is 10 kDa;

[0083] 3. Cultivation of stem cells: Active human placental mesenchymal stem cells were selected from the cell bank, cultured in phenol red-free DMEM medium at a temperature of 39°C and a carbon dioxide volume concentration of 6% to a growth density of 80%, washed the cells 4 times with PBS buffer, cultured in phenol red-free DMEM medium at a temperature of 39°C and a carbon dioxide volume concentration of 6% to a growth density of 95%, centrifuged the supernatant in the culture medium to obtain a supernatant containing exosomes, and filtered the supernatant containing exosomes using a filter membrane with a pore size of 0.22 μm to obtain the filtrate containing exosomes.

[0084] 4. Combination: 500 mL of exosomes, 14 g of carrier, and 260 mL of deionized water were mixed, and stirred at 500 rpm for 20 min at room temperature, 10 g of xanthan gum, 7 g of biological antibacterial agent, 4 g of sodium hyaluronate, 3 g of sodium carboxymethyl cellulose, and 2 g of polyvinyl alcohol 1788 were added, and the mixture was stirred for 2 h to obtain a stem cell composition;

[0085] The molecular weight of the sodium hyaluronate is 1000 kDa.

[0086] This embodiment also provides a stem cell composition for promoting skin wound healing prepared by the aforementioned preparation method.

[0087] Example 4

[0088] The preparation method of Example 2 is adjusted in that the compounding step (2) in the preparation of the carrier in step 1 is omitted, and the gel particles prepared in step (1) are used as carriers in the preparation of the combination in step 4.

[0089] Example 5

[0090] Adjustments were made to the preparation method of Example 2. The adjustments were as follows: in the compounding step (2) of the preparation of the carrier in step 1, the addition of gel particles was omitted, that is, calcium phosphate obtained by the reaction of calcium chloride and ammonium phosphate was directly used as the carrier.

[0091] Example 6

[0092] Adjustments were made to the preparation method of Example 2. The adjustments were as follows: the preparation of the inclusion complex in step (2) of the preparation of the biological antibacterial agent in step (2) was omitted, and the inclusion complex was replaced by an equal amount of the metal-organic framework material prepared in step (1) in the mixing in step (3), and the addition of low molecular weight zinc hyaluronate was omitted.

[0093] Test Example 1

[0094] Thirty-five male SD rats weighing 200-250 g were selected and randomly divided into 7 groups, 5 rats in each group, numbered 1-7. Each rat was anesthetized and fixed in a prone position, the hair on the back was shaved, and a punch with a diameter of 10 mm was used to press a circle on the back of the rat until it reached the fascia, and the skin was cut along the pressed circle to make a wound;

[0095] Immediately after the wounds were made, the stem cell compositions of Examples 1-6 were applied to the wounds of rats in Groups 1-6. The corresponding relationships are as follows:

[0096]

[0097] When applying, ensure that the stem cell composition can completely fill the wound, and use sterile gauze to bandage in the same way, then feed each rat in a cage, and treat the wound and replace the sterile gauze according to the above method every day. 7 groups of rats served as blank controls, without any treatment, and were directly fed in cages after the wound was made.

[0098] The wound conditions were recorded at 5d, 10d, 15d, and 20d after the wound was made. The results are as follows:

[0099]

[0100] It can be seen from the above results that the healing speed of the wounds of rats after using the stem cell compositions of Examples 5 and 6 is lower than that of Examples 1-4, and the wounds of rats after using the stem cell compositions of Examples 4-6 all show hyperplasia and thickening;

[0101] According to the analysis, in Example 4, only gel particles were used to load the growth factors, resulting in poor sustained-release ability of the prepared carrier and too rapid release of the growth factors, which led to hyperplasia and thickening of the rat wounds; in Example 5, only calcium phosphate was used to load the growth factors, which had limited loading capacity and poor sustained-release ability, and too rapid release of the growth factors, which led to hyperplasia and thickening of the rat wounds, and the chitosan in the gel particles could synergize with the growth factors in wound healing, and the addition of the gel particles was omitted, which slowed down the healing rate of the rat wounds; in Example 6, the use of metal-organic framework materials to encapsulate vitamin E was omitted, and the addition of small molecule hyaluronate zinc was also omitted, which has the effects of promoting wound healing and skin rejuvenation, thereby affecting the effect of the stem cell composition of Example 6.

[0102] Test Example 2

[0103] Thirty-five male SD rats weighing 200-250 g were selected and randomly divided into 7 groups, 5 rats in each group, numbered 1-7. Each rat was anesthetized and fixed in a prone position, the hair on the back was shaved, and a punch with a diameter of 10 mm was used to press a circle on the back of the rat until it reached the fascia, and the skin was cut along the pressed circle to make a wound;

[0104] After the wound was made, each rat was fed in a cage, and the wound was disinfected with medical alcohol three times a day. The scab formation of each rat's wound was observed and recorded. After the scab was formed on the rat, the stem cell composition of Examples 1-6 was immediately applied to the wound of the rat. The corresponding relationship is as follows:

[0105]

[0106] When applying, ensure that the stem cell composition can completely cover the wound surface, and use sterile gauze to bandage in the same way. Treat the wound surface and replace the sterile gauze every day according to the above method. Group 7 rats served as blank controls and did not receive any treatment after scab formation.

[0107] The skin recovery of each rat was recorded at 5d, 10d, and 15d after scab formation, and the results of each group were statistically analyzed. The statistical results are as follows:

[0108]

[0109] It can be seen from the above results that the healing speed of the rat wound after using the stem cell composition of Example 6 is lower than that of Examples 1-5;

[0110] According to analysis, Example 6 omits the use of metal-organic framework materials to encapsulate vitamin E, and also omits the addition of small molecule zinc hyaluronate. Vitamin E and small molecule zinc hyaluronate have good transdermal properties and can promote the skin's absorption of growth factors.

[0111] Test Example 3

[0112] Thirty-five male SD rats weighing 200-250 g were selected and randomly divided into 7 groups, 5 rats in each group, numbered 1-7. Each rat was anesthetized and fixed in a prone position, the hair on the back was shaved, and a punch with a diameter of 10 mm was used to press a circle on the back of the rat until it reached the fascia, and the skin was cut along the pressed circle to make a wound;

[0113] After the wound was made, each rat was fed in a separate cage, and 80 μL of 1×10 8 CFU / mL of Staphylococcus aureus liquid was added, and the wound was sealed with a sterile dressing. After the rat wound began to be infected, the Staphylococcus aureus liquid was added dropwise using the above method for 2 days, and then the addition of Staphylococcus aureus liquid was stopped, and the stem cell composition of Example 1-6 was immediately applied to the wound of the rat. The corresponding relationship is as follows:

[0114]

[0115] When applying, ensure that the stem cell composition can be completely filled in the wound, use sterile gauze to bandage in the same way, and treat the wound and replace the sterile gauze every day according to the above method. Group 7 rats served as blank controls and did not receive any treatment after stopping the dripping of Staphylococcus aureus liquid.

[0116] The skin recovery status of each rat was recorded 5 days, 10 days, 15 days, and 20 days after the application of the stem cell composition, and the results of each group were statistically analyzed. The statistical results are as follows:

[0117]

[0118] It can be seen from the above results that the wound healing speed and infection recovery speed of rats after using the stem cell composition of Examples 5-6 are lower than those of Examples 1-4;

[0119] According to analysis, Example 5 only uses calcium phosphate to load the growth factor, and no gel particles are added. The chitosan in the gel particles has an antibacterial effect, so Example 5 reduces the amount of antibacterial substances added, resulting in a slow recovery rate from infection, thereby affecting the wound healing rate; Example 6 omits the use of metal-organic framework materials to encapsulate vitamin E, and also omits the addition of small molecule hyaluronate zinc. Small molecule hyaluronate zinc has the advantages of good transdermal and bactericidal properties, so it can sterilize the skin surface and the inside of the skin. After omitting small molecule hyaluronate zinc, the bactericidal property of the stem cell composition becomes poor, further affecting the wound healing rate.

[0120] Unless otherwise specified, all percentages used in the present invention are by mass.

[0121] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a stem cell composition for promoting skin wound healing, characterized in that: The method comprises the following steps: preparing a carrier, preparing a biological antibacterial agent, culturing stem cells, and combining; The preparation of the carrier comprises the following steps: preparing gel particles, compounding; The method for preparing the gel particles comprises dissolving chitosan in an acetic acid aqueous solution, stirring at room temperature, adding a genipin aqueous solution, stirring at room temperature to obtain a dispersed phase; adding Span 80 to liquid paraffin, stirring at room temperature, adding the dispersed phase, shearing at room temperature, stirring at room temperature, adding anhydrous ethanol, continuing to stir at room temperature, centrifuging, washing, and drying the precipitate to obtain the gel particles; The composite comprises mixing the gel particles and deionized water, stirring at room temperature, adding a calcium chloride aqueous solution, continuing stirring, adjusting the pH to 9.5-10, and dropping an ammonium phosphate aqueous solution, and adjusting the pH to 9.5-10 during the dropping process. After the dropping is completed, centrifuging, washing, and drying the precipitate to obtain a carrier; The preparation of the biological antibacterial agent comprises the following steps: preparing a metal-organic framework material, preparing an inclusion compound, and mixing; The method for preparing the metal-organic framework material comprises mixing zinc chloride, β-cyclodextrin and deionized water, stirring at room temperature, adding anhydrous ethanol, continuing stirring, performing a hydrothermal reaction at 70-90° C., filtering, washing and drying the filter residue to obtain the metal-organic framework material; The preparation of the inclusion compound comprises mixing the metal-organic framework material and deionized water, stirring at room temperature, adding fat-soluble vitamin E, ultrasonically oscillating at room temperature, standing at room temperature for 10-12 hours, filtering, and drying the filter residue to obtain the inclusion compound; The mixing comprises mixing the gel particles obtained in the step of preparing the gel particles in the step of preparing the carrier, the inclusion compound, the low molecular weight hyaluronate zinc, and deionized water, stirring at room temperature, filtering, and drying the filter residue to obtain the biological antibacterial agent; The stem cells are cultured by selecting active human placental mesenchymal stem cells from a cell bank, culturing them in a phenol red-free DMEM medium at a temperature of 37-39° C. and a carbon dioxide volume concentration of 5-6% to a growth density of 75-80%, washing the cells 3-4 times with a PBS buffer, culturing them in a phenol red-free DMEM medium at a temperature of 37-39° C. and a carbon dioxide volume concentration of 5-6% to a growth density of 90-95%, centrifuging the supernatant in the culture medium to obtain a supernatant containing exosomes, and filtering the supernatant containing exosomes using a filter membrane with a pore size of 0.22 μm to obtain the filtrate containing exosomes; The combination comprises mixing exosomes, a carrier, and deionized water, stirring at room temperature, adding xanthan gum, a biological antibacterial agent, sodium hyaluronate, sodium carboxymethyl cellulose, and polyvinyl alcohol 1788, mixing, and continuing to stir to obtain a stem cell composition.

2. The method for preparing the stem cell composition for promoting skin wound healing according to claim 1, characterized in that: In the preparation of the gel particles, the mass volume ratio of chitosan, acetic acid aqueous solution, genipin aqueous solution, Span 80, liquid paraffin, and anhydrous ethanol is 1.8-2g:100-120mL:11-13mL:23-25mL:550-600mL:600-700mL; The mass concentration of the acetic acid aqueous solution is 1.4-1.6%; The mass concentration of the genipin aqueous solution is 0.5-0.6%.

3. The method for preparing the stem cell composition for promoting skin wound healing according to claim 1, characterized in that: The composite, gel particles, deionized water, calcium chloride aqueous solution, ammonium phosphate aqueous solution mass volume ratio is 20-25g:300-350mL:130-150mL:50-60mL; The mass concentration of the calcium chloride aqueous solution is 5%; The mass concentration of the ammonium phosphate aqueous solution is 4%; The dropping speed of the ammonium phosphate aqueous solution is 4-5 mL / min.

4. The method for preparing the stem cell composition for promoting skin wound healing according to claim 1, characterized in that: In the preparation of the metal-organic framework material, the mass volume ratio of zinc chloride, β-cyclodextrin, deionized water and anhydrous ethanol is 2.8-3g:11-13g:1000-1200mL:3.5-4mL.

5. The method for preparing the stem cell composition for promoting skin wound healing according to claim 4, characterized in that: In the preparation of the inclusion compound, the mass volume ratio of the metal-organic framework material, deionized water, and fat-soluble vitamin E is 3.5-3.7 g:100-105 mL:6.5-7.5 g.

6. The method for preparing the stem cell composition for promoting skin wound healing according to claim 5, characterized in that: In the mixing, the mass volume ratio of the gel particles prepared in the step of preparing the gel particles in the step of preparing the carrier, the inclusion compound, the low molecular weight hyaluronate zinc, and the deionized water is 200-210g:70-80g:20-25g:3000-3500mL.

7. The method for preparing the stem cell composition for promoting skin wound healing according to claim 1, characterized in that: In the combination, the mass volume ratio of exosomes, carrier, deionized water, xanthan gum, biological antibacterial agent, sodium hyaluronate, sodium carboxymethyl cellulose, and polyvinyl alcohol 1788 is 450-500 mL: 13-14 g: 240-260 mL: 8-10 g: 6-7 g: 3-4 g: 2-3 g: 1-2 g.

8. A stem cell composition for promoting skin wound healing, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7.