A method for manufacturing polyphenylene sulfide-based composite solid diaphragm by differential rolling

Through differential rolling technology and composite processing, the problem of poor thickness uniformity of polyphenylene sulfide solid separators has been solved, and a polyphenylene sulfide-based composite separator with high temperature resistance and ultra-thin characteristics has been achieved. It is suitable for a variety of ion batteries and reduces the cost of cost and expands the field of use.

CN118238445BActive Publication Date: 2024-10-22JIANGSU TONGLIN ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410195909.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-22
Publication Date
2024-10-22
Estimated Expiration
2044-02-22

AI Technical Summary

Technical Problem

The existing technology has problems such as poor thickness uniformity, inconsistent pole spacing, and easy breakage when rewinding when preparing polyphenylene sulfide solid separators. Moreover, the traditional hot rolling method cannot further reduce the thickness, which limits the use field of solid separators.

Method used

A method of manufacturing polyphenylene sulfide-based composite solid separators using differential rolling. Through the steps of powder making, blank making, film making and compounding, the differential rolling thinning technology of polyimide separators is used, combined with supporting diaphragms and glue. Through compound processing of liquid, an ultra-thin separator with uniform thickness and smooth surface is prepared.

Benefits of technology

The high-temperature resistance and ultra-thin characteristics of the polyphenylene sulfide-based composite solid separator are achieved, with a thickness of up to 5 μm. It is suitable for the field of ultra-thin solid separators, reduces costs, and improves the universal applicability of the separator.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118238445B_ABST
    Figure CN118238445B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of new energy materials, and specifically to a method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling. The specific steps include powder making, embryo making, film making and compounding; wherein in the film making stage, a polyimide diaphragm is introduced for hot pressing together, and the two rollers of the film making hot roller press form a differential speed, and the polyphenylene sulfide embryo roll is rolled to obtain a thinned polyphenylene sulfide solid diaphragm G; beneficial effects: the polyphenylene sulfide-based diaphragm obtained by the method has good high temperature resistance; by removing the metal chloride in the powder making process, the compressible film properties of the powder can be further improved, and by compounding different support films, it can be applied to lithium, sodium, zinc, and magnesium ion batteries, so that the diaphragm has universal applicability; the differential speed brought by the polyimide diaphragm is used to thin the embryo, the diaphragm has a uniform thickness, a smooth surface, no cracks, no large holes, and can further reduce the thickness of the diaphragm, so that it can be applied in the field of ultra-thin solid diaphragms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new energy materials, and in particular to a method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling. Background Art

[0002] With the excessive use of traditional fossil energy, environmental pollution and energy shortage are becoming increasingly serious. Some environmentally friendly and clean renewable energy sources have emerged. However, renewable energy sources such as solar energy, wind energy, and tidal energy are often intermittent and unstable, and cannot be directly connected to the grid and households, so their use is limited. As a solution, energy storage can store wind power and photovoltaic power and integrate it into the grid, which is considered to be a key link in the new power system. At present, in addition to traditional pumped energy storage, some new energy storage methods such as lithium-ion battery energy storage, sodium-ion battery energy storage, and aqueous zinc-ion battery energy storage are also used as new energy storage methods. As an important component of electrochemical energy storage batteries, diaphragms are crucial to the development of new energy storage methods. The diaphragm plays a role in blocking the direct contact between the positive and negative electrodes in the battery. On the other hand, the diaphragm needs to allow ions to pass stably while blocking the passage of electrons. The structure, porosity, and interaction between the diaphragm and the electrolyte significantly affect the ion transport of the diaphragm and the polarization of the battery.

[0003] Polyphenylene sulfide is a material with excellent heat resistance, chemical stability and insulation properties. The polyphenylene sulfide diaphragm (PPS) made by dry film forming has excellent electrochemical properties. Patent CN116001332A prepares polyphenylene sulfide diaphragm through conventional solvent-free dry electrode film forming technology, but has problems such as poor thickness uniformity, inconsistent inter-electrode spacing, and easy breakage of the tape during winding; CN116825941A and CN116988102A introduce a solvent semi-dry method and use traditional hot roller pressing, which can only press thick films with a thickness of more than 70μm and cannot be further thinned, limiting the application field of solid diaphragms.

[0004] Therefore, there is an urgent need for a production process that can optimize the preparation and compounding of polyphenylene sulfide solid diaphragms to improve the performance and continuous production capacity of polyphenylene sulfide solid diaphragms. Summary of the invention

[0005] The object of the present invention is to provide a method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling, so as to solve the problems raised in the above-mentioned background technology.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] Step 1: Powder preparation: (1) polyphenylene sulfide, tetrachlorobenzoquinone and deionized water are mixed to prepare mixed powder A; (2) the mixed powder A is subjected to a hydrothermal reaction to obtain powder B; (3) the powder B is mixed evenly with polytetrafluoroethylene powder at 0-5° C., and fiberized to obtain powder D;

[0008] Step 2: Blank making: Mix the powder D with alcohol and knead to obtain granular material E; press the granular material and dry it to obtain polyphenylene sulfide blank roll F;

[0009] Step 3: Film making: preheat the polyphenylene sulfide blank roll F, and perform differential rolling thinning on a film-making hot roller press together with the polyimide separator to obtain a polyphenylene sulfide solid separator G;

[0010] Step 4: Compounding: Dip the support diaphragm H into the glue solution I and compound it with the polyphenylene sulfide solid diaphragm G, dry, cut and roll it up to obtain a polyphenylene sulfide-based composite solid diaphragm.

[0011] Furthermore, during the powder making process, the mass ratio of polyphenylene sulfide, tetrachlorobenzoquinone and deionized water in the mixed powder A is (15-20):1:(5-8); the mass ratio of the polytetrafluoroethylene powder to the powder B is (90-95):(5-10); the hydrothermal reaction temperature is 150-250°C, and the reaction time is 2-10 hours;

[0012] Furthermore, in the embryo making process, the alcohol includes but is not limited to one or more of ethanol, 1,2-propylene glycol, glycerol, and isopropanol, the mass ratio of the powder D to the alcohol is (70-80): (20-30), the banburying time is 20-200 minutes, the size of the granular material E is 50 μm-5 mm; the roller surface temperature during the film pressing process is 30-120° C.; the drying temperature is 60-150° C., and the thickness of the polyphenylene sulfide embryo roll F is 100 μm-2 mm;

[0013] Furthermore, during the film-making process, the preheating temperature is 100-140° C., and the thickness of the polyimide membrane is 10-100 μm;

[0014] Furthermore, during the film making process, the two rollers of the film making hot roller press form a differential speed. The principle is that the speed difference between the two rollers is formed by controlling the speed of the roller surface covered by the polyimide diaphragm and the speed of the roller surface covered by the blank roll F. The speed ratio of the two rollers is 1:(1-5);

[0015] Furthermore, the thickness of the polyphenylene sulfide solid diaphragm G is 5-60 μm;

[0016] Furthermore, during the composite process, the supporting membrane H is a porous membrane, including but not limited to one of a polyethylene membrane, a polypropylene membrane, a cellulose membrane, a non-woven membrane, and a polyethylene terephthalate membrane, and has a thickness of 3-30 μm;

[0017] Furthermore, during the compounding process, the glue solution I is a mixture of an organic adhesive, an inorganic adhesive, an electrolyte salt and a solvent, and the mass ratio thereof is (4-5): (2-3): (42-43): (49-53); the organic adhesive includes but is not limited to one or more of polyvinyl alcohol, polyacrylate, and polytetrafluoroethylene; the inorganic adhesive includes but is not limited to one or more of sodium bentonite, lithium montmorillonite powder, and white carbon black; the electrolyte salt includes but is not limited to one or more of zinc trifluoromethanesulfonate, lithium bistrifluoromethanesulfonate imide, and sodium sulfate; the solvent includes but is not limited to one or more of deionized water, nitrogen methyl pyrrolidone, alcohol, and propylene glycol;

[0018] Furthermore, during the compounding process, the drying temperature is 30-120° C.; the thickness of the polyphenylene sulfide-based composite solid diaphragm is 15-200 μm, wherein the thickness of the adhesive layer formed by drying the adhesive solution I on the supporting diaphragm H is 100 nm-5 μm.

[0019] Compared with the prior art, the solid diaphragm prepared by the preparation process of the present invention has the following characteristics:

[0020] (1) The polyphenylene sulfide-based composite solid diaphragm manufactured by differential rolling in the application scheme has good high temperature resistance and does not shrink at 300°C;

[0021] (2) In the scheme, by removing the metal chloride in the mixed powder A during the powder making process in step 1, the compressible film properties of the powder can be further improved. By compounding different separators, it can be applied to lithium, sodium, zinc, and magnesium ion batteries, making the separator universal and further reducing the cost.

[0022] (3) The scheme uses the differential speed brought by the polyimide diaphragm to thin the blank. After thinning, the diaphragm has uniform thickness, smooth surface, no cracks, and no large holes. Compared with traditional same-speed rolling, differential hot rolling provides greater roller surface tangential friction, thereby providing higher shear force for polymer extension, making the diaphragm thinner. The minimum thickness can be 5μm, which can be used in the field of ultra-thin solid diaphragms. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The flow chart of differential film preparation using polyimide diaphragm;

[0024] Figure 2 This is a composite flow chart of polyphenylene sulfide diaphragm;

[0025] Figure 3 This is a picture of the polyphenylene sulfide solid diaphragm G after film formation in Example 1;

[0026] Figure 4 This is a picture of the polyphenylene sulfide-based composite solid diaphragm after compounding in Example 1. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the following examples, polyphenylene sulfide, manufacturer: Zhejiang Xinhecheng Co., Ltd.; tetrachlorobenzoquinone, manufacturer: Sinopharm Reagent; polytetrafluoroethylene, manufacturer: Chemours Teflon TM PTFE 601X; the content of 1,2-propylene glycol is 98%, manufacturer: Sinopharm Reagent; polyimide diaphragm, polyethylene diaphragm (5μm), manufacturer: Zhuhai Enjie; polyvinyl alcohol (molecular weight ~67000), sodium bentonite (particle size ~1250 mesh), zinc trifluoromethanesulfonate, manufacturer: Sinopharm Reagent; isopropanol, glycerol, nitrogen methyl pyrrolidone, polyacrylate (molecular weight ~25000), lithium montmorillonite powder (200 mesh), lithium bis(trifluoromethanesulfonic acid) amide, manufacturer: Sinopharm Reagent.

[0029] Example 1: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water are mixed to obtain mixed powder A, and the mixed powder A is placed in a closed reactor for hydrothermal reaction. The hydrothermal reaction atmosphere is air, the temperature is 200°C, the reaction time is 3 hours, and the hydrothermal reaction filling rate is 40%. After the reaction, the powder is washed to neutral and dried to obtain powder B.

[0030] The polytetrafluoroethylene powder and powder B are uniformly mixed in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state, specifically at 2°C. The powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in the powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0031] Powder D and 1,2-propylene glycol were mixed in a mass ratio of 75:25, and kneaded for 30 minutes to form granular material E, which was poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0032] The 50μm polyimide diaphragm is passed through the damping unwinding device through the film-making hot roller press, and the dried polyphenylene sulfide blank roll F is passed through the damping unwinding device into the preheating conveying rail for heating, and the blank roll F is heated to 130°C, and then fed into the film-making hot roller press, and hot-pressed together with the polyimide diaphragm. At this time, the temperature of the hot roller press is 135°C. The two rollers of the film-making hot roller press form a 1:3 differential speed, and the blank F is thinned under the hot pressing of the differential rollers. The polyimide diaphragm and the polyphenylene sulfide diaphragm are separated and rolled at the discharge port to obtain the finished polyphenylene sulfide solid diaphragm G, and the thickness of the polyphenylene sulfide solid diaphragm G is 20μm.

[0033] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite is carried out with the polyphenylene sulfide solid diaphragm G on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a polyethylene diaphragm (PE), and the glue I is composed of deionized water, polyvinyl alcohol, sodium bentonite and zinc trifluoromethane sulfonate in a mass ratio of 43:4.5:2.5:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, which is then rolled up. The temperature of the tunnel furnace is 30°C.

[0034] Example 2: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water are mixed to obtain mixed powder A, and the mixed powder A is charged into a closed reactor for hydrothermal reaction. The hydrothermal reaction atmosphere is air, the temperature is 200°C, the reaction time is 3 hours, and the hydrothermal reaction filling rate is 40%. After the reaction, the powder is washed to neutral and dried to obtain powder B.

[0035] The polytetrafluoroethylene powder and powder B are uniformly mixed in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state, specifically at 2°C. The powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in the powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0036] Powder D and isopropanol were mixed in a mass ratio of 75:25, and kneaded for 45 minutes to form granular material E, which was poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0037] The 50μm polyimide diaphragm is passed through the damping unwinding device through the film-making hot roller press, and the dried polyphenylene sulfide blank roll F is passed through the damping unwinding device into the preheating conveying rail for heating, and the blank roll F is heated to 130°C, and then fed into the film-making hot roller press, and hot-pressed together with the polyimide diaphragm. At this time, the temperature of the hot roller press is 135°C. The two rollers of the film-making hot roller press form a differential speed of 1:1.5, and the blank F is thinned under the hot pressing of the differential rollers. The polyimide diaphragm and the polyphenylene sulfide diaphragm are separated and rolled at the discharge port to obtain the finished polyphenylene sulfide solid diaphragm G, and the thickness of the polyphenylene sulfide solid diaphragm G is 30μm.

[0038] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite with the polyphenylene sulfide solid diaphragm G is performed on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a two-layer polypropylene diaphragm (PP), and the glue I is composed of deionized water, polyvinyl alcohol, sodium bentonite and zinc trifluoromethane sulfonate in a mass ratio of 43:5:2:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, which is then rolled up. The temperature of the tunnel furnace is 70°C.

[0039] Example 3: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water were mixed to prepare mixed powder A, and the mixed powder A was placed in a closed reactor for hydrothermal reaction. After the reaction, the powder was washed to neutral and dried to obtain powder B.

[0040] The polytetrafluoroethylene powder and powder B are uniformly mixed in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state, specifically at 2°C. The powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in the powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0041] Powder D and isopropanol were mixed in a mass ratio of 75:25, kneaded for 45 minutes to form granules E, which were poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0042] The 25μm polyimide diaphragm is passed through the damping unwinding device through the film-making hot roller press, and the dried polyphenylene sulfide blank roll F is passed through the damping unwinding device into the preheating conveying rail for heating, and the blank roll F is heated to 130°C, and then fed into the film-making hot roller press, and hot-pressed together with the polyimide diaphragm. At this time, the temperature of the hot roller press is 135°C. The two rollers of the film-making hot roller press form a differential speed of 1:1.5, and the blank F is thinned under the hot pressing of the differential rollers. The polyimide diaphragm and the polyphenylene sulfide diaphragm are separated and rolled at the discharge port to obtain the finished polyphenylene sulfide solid diaphragm G, and the thickness of the polyphenylene sulfide solid diaphragm G is 25μm.

[0043] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite is carried out with the polyphenylene sulfide solid diaphragm G on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a polyethylene diaphragm (PE), and the glue I is composed of deionized water, polyacrylate (PAA), lithium-based montmorillonite powder and lithium bistrifluoromethanesulfonic acid imide (LiTFSI) in a mass ratio of 43:4.5:2.5:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, and rolled up. The temperature of the tunnel furnace is 30°C.

[0044] Example 4: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water are mixed to obtain mixed powder A, and the mixed powder A is placed in a closed reactor for hydrothermal reaction. The hydrothermal reaction atmosphere is air, the temperature is 200°C, the reaction time is 3 hours, and the hydrothermal reaction filling rate is 40%. After the reaction, the powder is washed to neutral and dried to obtain powder B.

[0045] The polytetrafluoroethylene powder and powder B are mixed evenly in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out at a temperature where the polytetrafluoroethylene is in a glassy state, specifically at 2°C. Powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0046] Powder D was mixed with 1,2-propylene glycol in a mass ratio of 75:25, and kneaded for 45 minutes to form granular material E, which was poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0047] The 25μm polyimide diaphragm is passed through the damping unwinding device through the film-making hot roller press, and the dried polyphenylene sulfide blank roll F is passed through the damping unwinding device into the preheating conveying rail for heating, and the blank roll F is heated to 130°C, and then fed into the film-making hot roller press, and hot-pressed together with the polyimide diaphragm. At this time, the temperature of the hot roller press is 120°C. The two rollers of the film-making hot roller press form a differential speed of 1:1.5, and the blank F is thinned under the hot pressing of the differential rollers. The polyimide diaphragm and the polyphenylene sulfide diaphragm are separated and rolled at the discharge port to obtain the finished polyphenylene sulfide solid diaphragm G, and the thickness of the polyphenylene sulfide solid diaphragm G is 35μm.

[0048] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite is carried out with the polyphenylene sulfide solid diaphragm G on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a cellulose membrane, and the glue I is composed of deionized water, polyvinyl alcohol (PVA), sodium bentonite and zinc trifluoromethane sulfonate in a mass ratio of 42:5:3:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, which is then rolled up. The temperature of the tunnel furnace is 50°C.

[0049] Example 5: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water are mixed to prepare mixed powder A, and the mixed powder A is charged into a closed reactor for hydrothermal reaction. The hydrothermal reaction atmosphere is air, the temperature is 200°C, the reaction time is 3 hours, and the hydrothermal reaction filling rate is 40%. After the reaction, the powder is washed to neutral and dried to obtain powder B.

[0050] The polytetrafluoroethylene powder and powder B are uniformly mixed in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state, specifically at 2°C. The powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in the powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0051] Powder D and propylene glycol were mixed in a mass ratio of 75:25, kneaded for 2 hours to form granular material E, and poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0052] The 25μm polyimide diaphragm is passed through the damping unwinding device through the film-making hot roller press, and the dried polyphenylene sulfide blank roll F is passed through the damping unwinding device into the preheating conveying rail for heating, and the blank roll F is heated to 130°C, and then fed into the film-making hot roller press, and hot-pressed together with the polyimide diaphragm. At this time, the temperature of the hot roller press is 135°C. The two rollers of the film-making hot roller press form a differential speed of 1:5, and the blank F is thinned under the hot pressing of the differential rollers. The polyimide diaphragm and the polyphenylene sulfide diaphragm are separated and rolled at the discharge port to obtain the finished polyphenylene sulfide solid diaphragm G, and the thickness of the polyphenylene sulfide solid diaphragm G is 15μm.

[0053] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite is carried out with the polyphenylene sulfide solid diaphragm G on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a cellulose membrane, and the glue I is composed of nitrogen methyl pyrrolidone, polytetrafluoroethylene (PTFE), lithium montmorillonite powder and lithium bistrifluoromethylsulfonamide (LiTFSI) in a mass ratio of 43:4.5:2.5:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, and rolled up. The temperature of the tunnel furnace is 60°C.

[0054] Comparative Example 1: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water were mixed to prepare mixed powder A, and the mixed powder A was charged into a closed reactor for hydrothermal reaction. The hydrothermal reaction atmosphere was air, the temperature was 200°C, the reaction time was 3 hours, and the hydrothermal reaction filling rate was 40%. After the reaction, the powder was washed to neutral and dried to obtain powder B.

[0055] The polytetrafluoroethylene powder and powder B are uniformly mixed in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state, specifically at 2°C. The powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in the powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0056] Powder D and 1,2-propylene glycol were mixed in a mass ratio of 75:25, and kneaded for 30 minutes to form granular material E, which was poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0057] The dried polyphenylene sulfide stock roll F passes through the damping unwinding device and enters the preheating conveying guide rail for heating. The stock roll F is heated to 130°C and then fed into the film-making hot roller press. At this time, the temperature of the hot roller press is 135°C. The two rollers of the film-making hot roller press are at the same roller speed. The stock F is rolled to be thinned to obtain the finished polyphenylene sulfide solid diaphragm G. The thickness of the solid diaphragm G is 90μm.

[0058] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite is carried out with the polyphenylene sulfide solid diaphragm G on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a polyethylene diaphragm (PE), and the glue I is composed of deionized water, polyvinyl alcohol, sodium bentonite and zinc trifluoromethane sulfonate in a mass ratio of 43:4.5:2.5:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, which is then rolled up. The temperature of the tunnel furnace is 30°C.

[0059] Comparative Example 2: 3 kg of polyphenylene sulfide powder, 0.15 kg of tetrachlorobenzoquinone and 0.9 kg of deionized water were mixed to prepare mixed powder A, and the mixed powder A was charged into a closed reactor for hydrothermal reaction. The hydrothermal reaction atmosphere was air, the temperature was 200°C, the reaction time was 3 hours, and the hydrothermal reaction filling rate was 40%. After the reaction, the powder was washed to neutral and dried to obtain powder B.

[0060] The polytetrafluoroethylene powder and powder B are uniformly mixed in a mixer at a mass ratio of 94:6 to obtain powder C. The mixing process is carried out under the temperature condition that the polytetrafluoroethylene is in a glassy state, specifically at 2°C. The powder C is subjected to fiberization treatment by a supersonic jet of dry air, so that the molecular chains of the polytetrafluoroethylene in the powder C are extended and opened, forming a physical bond with the powder in B without chemical reaction, thereby obtaining powder D.

[0061] Powder D and 1,2-propylene glycol were mixed in a mass ratio of 75:25, and kneaded for 30 minutes to form granular material E, which was poured into the feeding system of a horizontal hot roller press for film pressing to form a continuous polyphenylene sulfide blank roll F, which was placed in an oven at 100°C for complete drying.

[0062] The 25μm polyimide membrane is passed through the damping unwinding device through the film-making hot roller press, and the dried polyphenylene sulfide stock roll F is passed through the damping unwinding device into the preheating conveying rail for heating, and the stock roll F is heated to 130°C, and then fed into the film-making hot roller press, and hot-pressed together with the polyimide membrane. At this time, the temperature of the hot roller press is 135°C. The stock F is thinned under the same speed hot roller press, and the polyimide membrane and the polyphenylene sulfide membrane are separated and rolled at the discharge port to obtain the finished polyphenylene sulfide solid membrane G, and the thickness of the polyphenylene sulfide solid membrane G is 75μm.

[0063] The polyphenylene sulfide solid diaphragm G enters the laminating machine through the guide rail, the supporting diaphragm H passes through the glue tank storing the glue I to pick up the glue I, and the excess glue is scraped off by the scraper, and the composite is carried out with the polyphenylene sulfide solid diaphragm G on the platform, and then the composite of the supporting diaphragm H and the polyphenylene sulfide solid diaphragm G is completed by rolling. At this time, the supporting diaphragm H is a polyethylene diaphragm (PE), and the glue I is composed of deionized water, polyvinyl alcohol, sodium bentonite and zinc trifluoromethane sulfonate in a mass ratio of 43:4.5:2.5:50. The composite diaphragm is dried in a tunnel furnace and then cut to obtain the finished polyphenylene sulfide-based composite solid diaphragm, which is then rolled up. The temperature of the tunnel furnace is 30°C.

[0064] Experiment: Measure the thickness of the polyphenylene sulfide solid diaphragm G of Examples 1-5 and Comparative Examples 1-2; Take the finished composite solid diaphragm and measure the thickness of its adhesive layer; Cut out a 3cm×3cm standard square from the finished diaphragm, heat it to 300°C, remeasure its length and width, and calculate the overall shrinkage rate. The specific data are shown in the following table:

[0065]

[0066] Conclusion: The experimental data of Examples 1-5 and Comparative Examples 1-2 show that the polyphenylene sulfide-based solid diaphragm manufactured by differential rolling is thinner in thickness and adhesive layer thickness than the diaphragm manufactured by conventional rolling. At 300°C, the diaphragm manufactured by conventional rolling has a higher shrinkage rate, while the diaphragm obtained by differential rolling has better high temperature resistance and stability.

[0067] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling, characterized in that: The following steps are involved: Step 1: Powder preparation: (1) polyphenylene sulfide, tetrachlorobenzoquinone and deionized water are mixed to form a mixed powder A; (2) subjecting the mixed powder A to a hydrothermal reaction to obtain powder B; (3) uniformly mixing powder B with polytetrafluoroethylene powder, and fiberizing the mixture to obtain powder D; Step 2: Blank making: Mix the powder D with alcohol and knead to obtain granular material E; press the granular material and dry it to obtain polyphenylene sulfide blank roll F; Step 3: Film making: preheat the polyphenylene sulfide blank roll F at 100-140°C, and perform differential rolling thinning on a film-making hot roller press together with a polyimide separator, wherein the two rollers form a differential speed, and the speed ratio of the two rollers is 1:(1.5-5), to obtain a polyphenylene sulfide solid separator G; Step 4: Compounding: Dip the support diaphragm H into the glue solution I and compound it with the polyphenylene sulfide solid diaphragm G, dry, cut and roll it up to obtain a polyphenylene sulfide-based composite solid diaphragm; The thickness of the polyimide diaphragm is 10-100 μm; the thickness of the polyphenylene sulfide solid diaphragm G is 5-60 μm.

2. The method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling according to claim 1, characterized in that: During the powder making process, the mass ratio of polyphenylene sulfide, tetrachlorobenzoquinone and deionized water in the mixed powder A is (15-20):1:(5-8); the mass ratio of the polytetrafluoroethylene powder to the powder B is (90-95):(5-10); the hydrothermal reaction temperature is 150-250°C, and the reaction time is 2-10 hours.

3. The method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling according to claim 1, characterized in that: During the embryo making process, the alcohol includes one or more of ethanol, 1,2-propylene glycol, glycerol, and isopropanol, the mass ratio of the powder D to the alcohol is (70-80): (20-30), the mixing time is 20-200 minutes, and the size of the granular material E is 50μm-5mm; the roller surface temperature during the film pressing process is 30-120°C; the drying temperature is 60-150°C, and the thickness of the polyphenylene sulfide embryo roll F is 100μm-2mm.

4. The method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling according to claim 1, characterized in that: During the compounding process, the supporting membrane H is a porous membrane, including one of a polyethylene membrane, a polypropylene membrane, a cellulose membrane, a non-woven fabric membrane, and a polyethylene terephthalate membrane, and has a thickness of 3-30 μm.

5. The method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling according to claim 1, characterized in that: During the compounding process, the glue solution I is a mixture of a solvent, an organic adhesive, an inorganic adhesive and an electrolyte salt, and the mass ratio thereof is (42-43): (4-5): (2-3): (49-53); the organic adhesive includes one or more of polyvinyl alcohol, polyacrylate, and polytetrafluoroethylene; the inorganic adhesive includes one or more of sodium bentonite, lithium montmorillonite powder, and white carbon black; the electrolyte salt includes one or more of zinc trifluoromethanesulfonate, lithium bistrifluoromethanesulfonate imide, and sodium sulfate; the solvent includes one or more of deionized water, nitrogen methyl pyrrolidone, alcohol, and propylene glycol.

6. The method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling according to claim 1, characterized in that: During the compounding process, the drying temperature is 30-120° C.; the thickness of the polyphenylene sulfide-based composite solid diaphragm is 15-200 μm, and the thickness of the adhesive layer formed by drying the adhesive solution I on the supporting diaphragm H is 100 nm-5 μm. 7 . The polyphenylene sulfide-based composite solid diaphragm prepared by the method for manufacturing a polyphenylene sulfide-based composite solid diaphragm by differential rolling according to any one of claims 1 to 6 .