A method for preparing a high thermal conductivity flake graphite / copper composite material
Through the coating of nano-scale chromium carbide layer and liquid phase extrusion technology, the problem of poor bonding between scale graphite and copper is solved, and a high thermal conductivity and low density scale graphite/copper composite material is achieved, which improves the two-dimensional heat of the material Conductivity and density meet the heat dissipation needs of electronic devices.
Patent Information
- Application Number
- CN202410343601.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-25
AI Technical Summary
The existing scale graphite/copper composite materials have poor interface bonding between copper and scale graphite, resulting in a decrease in thermal conductivity, and the directional arrangement of scale graphite is difficult, affecting the high thermal conductivity of the material.
By pretreating the scale graphite, coating the nanoscale chromium carbide layer, and using liquid phase extrusion and air pressure impregnation technology, a highly oriented scale graphite/copper composite material is formed to improve interface bonding and material density.
It realizes high thermal conductivity and low density flake graphite/copper composite materials, which improves the two-dimensional thermal conductivity and density of the material and meets the heat dissipation needs of electronic devices.
Smart Images

Figure CN118241071B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a flake graphite / copper composite material. Background Art
[0002] As the power and assembly density of electronic devices increase, good heat dissipation is crucial to improving device performance and extending device life, especially for small-volume mobile devices that rely on passive heat dissipation. However, traditional metal materials have certain limitations in terms of high heat dissipation performance requirements and matching the thermal expansion coefficient of semiconductor chips. Therefore, there is a strong market demand for a new generation of high thermal conductivity electronic packaging materials.
[0003] Flake graphite has a distinct lamellar structure, high two-dimensional thermal conductivity and relatively low thermal expansion coefficient. my country has abundant graphite resources, which are low-cost and high-quality. Currently, flake graphite has been widely used as a reinforcement in metal-based composites. Since flake graphite exhibits excellent thermal conductivity in the plane, it is combined with copper, which has good thermal conductivity, to prepare flake graphite / copper composite materials that show excellent thermal conductivity potential.
[0004] At present, the preparation of flake graphite / copper composite materials is mainly based on the solid phase method (hot pressing sintering, spark plasma sintering), but the composite materials prepared by the solid phase method have low density, resulting in a decrease in the thermal conductivity of the material. The composite materials prepared by the liquid phase method have higher density, but due to the chemical inertness and poor wettability between copper and flake graphite, how to improve the interface bonding between copper and flake graphite has become an important issue in the preparation of flake graphite / copper composite materials by the liquid phase method.
[0005] In addition, the key to fully exerting the thermal conductivity of flake graphite in composite materials is to achieve directional arrangement of flake graphite. Flake graphite is in the form of thin flakes, has small particle size, is lightweight, and is easily broken. Therefore, it is difficult to directly achieve high orientation of flake graphite through direct extrusion or vibration. This has also become a key issue that needs to be solved in the preparation of flake graphite / copper composite materials. Summary of the invention
[0006] In order to solve the problems of chemical inertness and poor wettability between existing copper and flake graphite, and difficulty in oriented arrangement of flake graphite, the present invention provides a method for preparing a high thermal conductivity flake graphite / copper composite material.
[0007] The preparation method of the high thermal conductivity flake graphite / copper composite material of the present invention is carried out according to the following steps:
[0008] 1. Pretreatment: Take the flakes and sieve them, then put the flake graphite into a 10% NaOH solution by mass, soak it at 80°C for 10 minutes, then filter out the flake graphite and wash it with deionized water until it is neutral, then soak it in a 10% HCl solution by mass for 10 minutes, finally filter out the flake graphite and wash it with deionized water until it is neutral, and dry it for use;
[0009] 2. Preparation of coating: Put the flake graphite pretreated in step 1 into a NaCl-KCl-Cr mixed salt, mix it evenly with a mixer, put it in a crucible, and heat it under a protective atmosphere to obtain chromium carbide plated flake graphite;
[0010] The NaCl-KCl-Cr mixed salt is a mixture of powdered NaCl, powdered KCl and Cr powder. In the NaCl-KCl-Cr mixed salt, the mass fractions of NaCl, KCl and Cr are x, y and z respectively, wherein x=y, 5%≤z≤25%;
[0011] The heating process is: keeping the temperature at 800-1000°C for 10-360 minutes;
[0012] 3. Preparation of preform: Mix chromium carbide-coated flake graphite with anhydrous ethanol and place in a crucible, use a pressing plate to squeeze the mixture in the crucible, keep squeezing and invert the crucible to dry, and obtain a stacked high-oriented chromium carbide-coated flake graphite preform;
[0013] The mass of the anhydrous ethanol is 20%-80% of the mass of the flake graphite;
[0014] The extrusion pressure is 50-400N;
[0015] 4. Gas pressure infiltration: Place the extrusion crucible upright, weigh the pure copper ingot and place it on the top of the crucible, then transfer it to the infiltration furnace, evacuate the infiltration furnace to vacuum, and finally heat it up and fill it with protective gas for gas pressure infiltration;
[0016] The heating temperature is 1050-1200°C;
[0017] During the gas pressure infiltration process, the protective gas pressure is 15-25 MPa and the insulation time is 1-6 hours.
[0018] The principles and beneficial effects of the present invention are:
[0019] The composite material prepared by the present invention has the characteristics of high orientation, high density, high thermal conductivity and low density, and can meet the performance requirements of heat dissipation materials in electronic devices. First, the flake graphite is pretreated, and then a nano-scale chromium carbide coating is plated on the surface of the flake graphite by a molten salt method, and a high-oriented flake graphite preform is obtained by liquid phase extrusion. Finally, a flake graphite / copper composite material with high density and high orientation is prepared by air pressure infiltration, which has the following beneficial effects:
[0020] 1. The present invention uses a molten salt method to plate a nano-scale chromium carbide coating on the surface of flake graphite, thereby avoiding direct contact between copper and carbon, solving the problem of non-wetting between copper and carbon, improving the interface bonding between flake graphite and matrix copper, reducing the difficulty of infiltration, and promoting the molding of composite materials. In addition, a thinner chromium carbide coating can reduce the interface thermal resistance and improve the overall thermal conductivity of the composite material.
[0021] 2. The present invention uses liquid phase extrusion, and compared with the natural stacking of flake graphite in the air, flake graphite is easy to disperse and spread in the liquid phase, and a greater pressure can be applied during the extrusion process so that the flake graphite forms a preferential orientation under pressure, thereby improving the orientation of the flake graphite in the mold before infiltration, and thus can improve the two-dimensional thermal conductivity of the composite material prepared using the flake graphite.
[0022] 3. The present invention uses gas pressure infiltration equipment to infiltrate liquid copper into a crucible filled with flake graphite at high temperature, and achieves a close combination of copper and flake graphite through gas pressure. Compared with the solid phase method, the porosity of the prepared composite material is significantly reduced, which is beneficial to the improvement of the thermal conductivity of the material.
[0023] 4. The present invention can realize the preparation of flake graphite / copper composite materials with different volume fractions by adjusting the liquid phase extrusion pressure to meet the material requirements of different densities and thermal conductivities.
[0024] 5. The present invention has no requirements on the size of flake graphite. High orientation of flake graphite of different sizes can be achieved through liquid phase extrusion, and flake graphite / copper composite materials of different sizes and flake graphite / copper composite materials of multiple sizes can be prepared. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM photo of the high thermal conductivity flake graphite / copper composite material obtained in Example 1;
[0026] Figure 2 This is a SEM photo of the high thermal conductivity flake graphite / copper composite material obtained in Example 2. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any reasonable combination of the specific implementation modes.
[0028] Specific implementation method 1: The preparation method of the high thermal conductivity flake graphite / copper composite material of this implementation method is carried out according to the following steps:
[0029] 1. Pretreatment: Take the flakes and sieve them, then put the flake graphite into a 10% NaOH solution by mass, soak it at 80°C for 10 minutes, then filter out the flake graphite and wash it with deionized water until it is neutral, then soak it in a 10% HCl solution by mass for 10 minutes, finally filter out the flake graphite and wash it with deionized water until it is neutral, and dry it for use;
[0030] 2. Preparation of coating: Put the flake graphite pretreated in step 1 into a NaCl-KCl-Cr mixed salt, mix it evenly with a mixer, put it in a crucible, and heat it under a protective atmosphere to obtain chromium carbide plated flake graphite;
[0031] The NaCl-KCl-Cr mixed salt is a mixture of powdered NaCl, powdered KCl and Cr powder. In the NaCl-KCl-Cr mixed salt, the mass fractions of NaCl, KCl and Cr are x, y and z respectively, wherein x=y, 5%≤z≤25%;
[0032] The heating process is: keeping the temperature at 800-1000°C for 10-360 minutes;
[0033] 3. Preparation of preform: Mix chromium carbide-coated flake graphite with anhydrous ethanol and place in a crucible, use a pressing plate to squeeze the mixture in the crucible, keep squeezing and invert the crucible to dry, and obtain a stacked high-oriented chromium carbide-coated flake graphite preform;
[0034] The mass of the anhydrous ethanol is 20%-80% of the mass of the flake graphite;
[0035] The extrusion pressure is 50-400N;
[0036] 4. Gas pressure infiltration: Place the extrusion crucible upright, weigh the pure copper ingot and place it on the top of the crucible, then transfer it to the reactor, evacuate the reactor to vacuum, and finally heat it up and fill it with protective gas for gas pressure infiltration;
[0037] The heating temperature is 1050-1200°C;
[0038] During the gas pressure infiltration process, the protective gas pressure is 15-25 MPa and the insulation time is 1-6 hours.
[0039] The composite material prepared in this embodiment has the characteristics of high orientation, high density, high thermal conductivity and low density, and can meet the performance requirements of heat dissipation materials in electronic devices. First, the flake graphite is pretreated, and then a nano-scale chromium carbide coating is plated on the surface of the flake graphite by a molten salt method, and a high-oriented flake graphite preform is obtained by liquid phase extrusion. Finally, a flake graphite / copper composite material with high density and high orientation is prepared by air pressure infiltration, which has the following characteristics:
[0040] Beneficial effects:
[0041] 1. This embodiment uses a molten salt method to plate a nano-scale chromium carbide coating on the surface of flake graphite, avoiding direct contact between copper and carbon, solving the problem of copper and carbon not wetting, improving the interface bonding between flake graphite and matrix copper, reducing the difficulty of infiltration, and promoting the molding of composite materials. In addition, a thinner chromium carbide coating can reduce the interface thermal resistance and improve the overall thermal conductivity of the composite material.
[0042] 2. This embodiment uses liquid phase extrusion. Compared with the natural stacking of flake graphite in the air, flake graphite is easy to disperse and spread in the liquid phase, and a greater pressure can be applied during the extrusion process so that the flake graphite forms a preferential orientation under pressure, thereby improving the orientation of the flake graphite in the mold before infiltration, and thus can improve the two-dimensional thermal conductivity of the composite material prepared using the flake graphite.
[0043] 3. In this embodiment, liquid copper is infiltrated into a crucible filled with flake graphite at high temperature through gas pressure infiltration equipment, and a close combination of copper and flake graphite is achieved through gas pressure. Compared with the solid phase method, the porosity of the prepared composite material is significantly reduced, which is beneficial to the improvement of the thermal conductivity of the material.
[0044] 4. This embodiment can achieve the preparation of flake graphite / copper composite materials with different volume fractions by adjusting the liquid phase extrusion pressure to meet the material requirements of different densities and thermal conductivities.
[0045] 5. This embodiment has no requirements on the size of flake graphite. High orientation of flake graphite of different sizes can be achieved through liquid phase extrusion, and flake graphite / copper composite materials of different sizes and flake graphite / copper composite materials of multiple sizes can be prepared.
[0046] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the particle size of the flake graphite after sieving in step 1 is 250 to 2000 μm.
[0047] Specific implementation method three: This implementation method is different from specific implementation methods one or two in that: the NaCl-KCl-Cr mixed salt powder NaCl, powder KCl and Cr powder described in step two are mixed, and the mass fractions of NaCl, KCl and Cr in the NaCl-KCl-Cr mixed salt are 45%, 45% and 10% respectively.
[0048] Specific implementation method 4: This implementation method is different from any one of specific implementation methods 1 to 3 in that: the rotation speed of the mixer in step 2 is 50 to 300 rpm, and the mixing time is 3 to 24 hours.
[0049] Specific implementation mode 5: This implementation mode is different from any one of specific implementation modes 1 to 4 in that: the protective atmosphere in step 2 is an argon atmosphere, a nitrogen atmosphere or a helium atmosphere.
[0050] Specific implementation method 6: This implementation method is different from any one of specific implementation methods 1 to 5 in that: the heating process in step 2 is: keeping the temperature at 920° C. for 20 minutes.
[0051] Specific implementation method 7: This implementation method is different from any one of specific implementation methods 1 to 6 in that: the mass of the anhydrous ethanol in step 3 is 80% of the mass of the flake graphite.
[0052] Specific implementation eight: This implementation differs from any one of specific implementations one to seven in that: the volume of the pure copper ingot in step four is 1.5 times that of the chromium carbide plated flake graphite preform.
[0053] Specific implementation method 9: This implementation method is different from any one of specific implementation methods 1 to 8 in that: the impregnation furnace described in step 4 is evacuated to a vacuum degree of 1-10Pa.
[0054] Specific implementation method ten: This implementation method is different from any one of specific implementation methods one to nine in that: the protective gas in step four is argon, nitrogen or helium.
[0055] Example 1
[0056] The preparation method of the high thermal conductivity flake graphite / copper composite material of this embodiment is carried out according to the following steps:
[0057] 1. Pretreatment: Take the flakes and sieve them, then put the flake graphite into a 10% NaOH solution by mass, soak it at 80°C for 10 minutes, then filter out the flake graphite and wash it with deionized water until it is neutral, then soak it in a 10% HCl solution by mass for 10 minutes, finally filter out the flake graphite and wash it with deionized water until it is neutral, and dry it for use;
[0058] The particle size of the sieved flake graphite is 450-550 μm;
[0059] 2. Preparation of coating: Put the flake graphite pretreated in step 1 into a NaCl-KCl-Cr mixed salt, mix it evenly with a mixer, put it in a crucible, and heat it under a protective atmosphere to obtain chromium carbide plated flake graphite;
[0060] The NaCl-KCl-Cr mixed salt is formed by mixing powdered NaCl, powdered KCl and Cr powder, wherein the mass fractions of NaCl, KCl and Cr in the NaCl-KCl-Cr mixed salt are 45%, 45% and 10% respectively;
[0061] The speed of the mixer is 50 rpm and the mixing time is 6 h;
[0062] The protective atmosphere is a helium atmosphere;
[0063] The heating process is: keeping the temperature at 920°C for 20 minutes;
[0064] 3. Preparation of preform: Mix chromium carbide-coated flake graphite with anhydrous ethanol and place in a crucible, use a pressing plate to squeeze the mixture in the crucible, keep squeezing and invert the crucible to dry, and obtain a stacked high-oriented chromium carbide-coated flake graphite preform;
[0065] The mass of the anhydrous ethanol is 40% of the mass of the flake graphite;
[0066] The extrusion pressure is 200N;
[0067] 4. Gas pressure infiltration: Place the extrusion crucible upright, weigh the pure copper ingot and place it on the top of the crucible, then transfer it to the infiltration furnace, evacuate the infiltration furnace to vacuum, and finally heat it up and fill it with protective gas for gas pressure infiltration;
[0068] The heating temperature is 1050°C;
[0069] The impregnation furnace is evacuated to a vacuum degree of 1 Pa;
[0070] During the gas pressure infiltration process, the protective gas pressure is 20MPa and the insulation time is 2h;
[0071] The protective gas is nitrogen.
[0072] Figure 1 This is a SEM photo of the high thermal conductivity flake graphite / copper composite material obtained in Example 1. It can be seen that the flake graphite is evenly distributed in the matrix, arranged in an orderly manner, and oriented in a nearly consistent manner, so that the composite material has a high two-dimensional thermal conductivity. The average density of the flake graphite / copper composite material prepared in Example 1 is 4.96 g / cm 3 , the thermal conductivity in the XY plane is 587W / (m·K).
[0073] Example 2
[0074] The preparation method of the high thermal conductivity flake graphite / copper composite material of this embodiment is carried out according to the following steps:
[0075] 1. Pretreatment: Take the flakes and sieve them, then put the flake graphite into a 10% NaOH solution by mass, soak it at 80°C for 10 minutes, then filter out the flake graphite and wash it with deionized water until it is neutral, then soak it in a 10% HCl solution by mass for 10 minutes, finally filter out the flake graphite and wash it with deionized water until it is neutral, and dry it for use;
[0076] The particle size of the sieved flake graphite is 450-550 μm;
[0077] 2. Preparation of coating: Put the flake graphite pretreated in step 1 into a NaCl-KCl-Cr mixed salt, mix it evenly with a mixer, put it in a crucible, and heat it under a protective atmosphere to obtain chromium carbide plated flake graphite;
[0078] The NaCl-KCl-Cr mixed salt is a mixture of powdered NaCl, powdered KCl and Cr powder, wherein the mass fractions of NaCl, KCl and Cr in the NaCl-KCl-Cr mixed salt are 40%, 40% and 20% respectively;
[0079] The speed of the mixer is 50 rpm and the mixing time is 6 h;
[0080] The protective atmosphere is a nitrogen atmosphere;
[0081] The heating process is: keeping the temperature at 950°C for 10 minutes;
[0082] 3. Preparation of preform: Mix chromium carbide-coated flake graphite with anhydrous ethanol and place in a crucible, use a pressing plate to squeeze the mixture in the crucible, keep squeezing and invert the crucible to dry, and obtain a stacked high-oriented chromium carbide-coated flake graphite preform;
[0083] The mass of the anhydrous ethanol is 40% of the mass of the flake graphite;
[0084] The extrusion pressure is 200N;
[0085] 4. Gas pressure infiltration: Place the extrusion crucible upright, weigh the pure copper ingot and place it on the top of the crucible, then transfer it to the infiltration furnace, evacuate the infiltration furnace to vacuum, and finally heat it up and fill it with protective gas for gas pressure infiltration;
[0086] The volume of the pure copper ingot is 1.5 times that of the chromium carbide plated flake graphite preform;
[0087] The heating temperature is 1050°C;
[0088] The impregnation furnace is evacuated to a vacuum degree of 1 Pa;
[0089] During the gas pressure infiltration process, the protective gas pressure is 20MPa and the insulation time is 1.5h;
[0090] The protective gas is nitrogen.
[0091] Figure 2 This is a SEM photo of the high thermal conductivity flake graphite / copper composite material obtained in Example 2. It can be seen that the flake graphite is evenly distributed in the matrix, arranged in an orderly manner, and has a nearly consistent orientation, so that the composite material has a high two-dimensional thermal conductivity.
[0092] Example 2: The average density of the flake graphite / copper composite material prepared was 5.2 g / cm 3 , the thermal conductivity in the XY plane is 537W / (m·K).
[0093] Example 3
[0094] The preparation method of the high thermal conductivity flake graphite / copper composite material of this embodiment is carried out according to the following steps:
[0095] 1. Pretreatment: Take the flakes and sieve them, then put the flake graphite into a 10% NaOH solution by mass, soak it at 80°C for 10 minutes, then filter out the flake graphite and wash it with deionized water until it is neutral, then soak it in a 10% HCl solution by mass for 10 minutes, finally filter out the flake graphite and wash it with deionized water until it is neutral, and dry it for use;
[0096] The particle size of the sieved flake graphite is 450-550 μm;
[0097] 2. Preparation of coating: Put the flake graphite pretreated in step 1 into a NaCl-KCl-Cr mixed salt, mix it evenly with a mixer, put it in a crucible, and heat it under a protective atmosphere to obtain chromium carbide plated flake graphite;
[0098] The NaCl-KCl-Cr mixed salt is a mixture of powdered NaCl, powdered KCl and Cr powder, wherein the mass fractions of NaCl, KCl and Cr in the NaCl-KCl-Cr mixed salt are 40%, 40% and 20% respectively;
[0099] The speed of the mixer is 50 rpm and the mixing time is 6 h;
[0100] The protective atmosphere is a nitrogen atmosphere;
[0101] The heating process is: keeping the temperature at 920°C for 20 minutes;
[0102] 3. Preparation of preform: Mix chromium carbide-coated flake graphite with anhydrous ethanol and place in a crucible, use a pressing plate to squeeze the mixture in the crucible, keep squeezing and invert the crucible to dry, and obtain a stacked high-oriented chromium carbide-coated flake graphite preform;
[0103] The mass of the anhydrous ethanol is 40% of the mass of the flake graphite;
[0104] The extrusion pressure is 200N;
[0105] 4. Gas pressure infiltration: Place the extrusion crucible upright, weigh the pure copper ingot and place it on the top of the crucible, then transfer it to the infiltration furnace, evacuate the infiltration furnace to vacuum, and finally heat it up and fill it with protective gas for gas pressure infiltration;
[0106] The volume of the pure copper ingot is 1.5 times that of the chromium carbide plated flake graphite preform;
[0107] The heating temperature is 1050°C;
[0108] The impregnation furnace is evacuated to a vacuum degree of 1.5 Pa;
[0109] During the gas pressure infiltration process, the protective gas pressure is 20MPa and the insulation time is 1.5h;
[0110] The protective gas is nitrogen.
[0111] Example 3: The average density of the flake graphite / copper composite material prepared was 4.68 g / cm 3 , the thermal conductivity in the XY plane is 527W / (m·K).
Claims
1. A method for preparing a high thermal conductivity flake graphite / copper composite material, characterized in that: The preparation method of the high thermal conductivity flake graphite / copper composite material is carried out according to the following steps:
1. Pretreatment: Take the flakes and sieve them, then put the flake graphite into a 10% NaOH solution by mass, soak it at 80°C for 10 minutes, then filter out the flake graphite and wash it with deionized water until it is neutral, then soak it in a 10% HCl solution by mass for 10 minutes, finally filter out the flake graphite and wash it with deionized water until it is neutral, and dry it for use; 2. Preparation of coating: Put the flake graphite pretreated in step 1 into a NaCl-KCl-Cr mixed salt, mix it evenly with a mixer, put it in a crucible, and heat it under a protective atmosphere to obtain chromium carbide plated flake graphite; The NaCl-KCl-Cr mixed salt is prepared by mixing powdered NaCl, powdered KCl and Cr powder. In the NaCl-KCl-Cr mixed salt, the mass fractions of NaCl, KCl and Cr are x, y and z respectively, wherein x=y, 5%≤z≤25%; The heating process is: keeping the temperature at 800-1000°C for 10-360 minutes; 3. Preparation of preform: Mix chromium carbide-coated flake graphite with anhydrous ethanol and place in a crucible, use a pressing plate to squeeze the mixture in the crucible, keep squeezing and invert the crucible to dry, and obtain a stacked high-oriented chromium carbide-coated flake graphite preform; The mass of the anhydrous ethanol is 20%-80% of the mass of the flake graphite; The extrusion pressure is 50-400N; 4. Gas pressure infiltration: Place the extrusion crucible upright, weigh the pure copper ingot and place it on the top of the crucible, then transfer it to the reactor, evacuate the reactor to vacuum, and finally heat it up and fill it with protective gas for gas pressure infiltration; The heating temperature is 1050-1200°C; During the gas pressure infiltration process, the protective gas pressure is 15-25 MPa and the insulation time is 1-6 hours.
2. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: The particle size of the flake graphite after sieving in step 1 is 250 to 2000 μm.
3. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: Step 2: The NaCl-KCl-Cr mixed salt is prepared by mixing powdered NaCl, powdered KCl and Cr powder. In the NaCl-KCl-Cr mixed salt, the mass fractions of NaCl, KCl and Cr are 45%, 45% and 10% respectively.
4. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: In step 2, the rotating speed of the mixer is 50 to 300 rpm, and the mixing time is 3 to 24 hours.
5. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: The protective atmosphere in step 2 is argon atmosphere, nitrogen atmosphere or helium atmosphere.
6. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: The heating process in step 2 is: keeping the temperature at 920° C. for 20 minutes.
7. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: The mass of the anhydrous ethanol in step 3 is 80% of the mass of the flake graphite.
8. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: The volume of the pure copper ingot in step 4 is 1.5 times that of the chromium carbide plated flake graphite preform.
9. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: In step 4, the reactor is evacuated to a vacuum degree of 1-10Pa.
10. The method for preparing the high thermal conductivity flake graphite / copper composite material according to claim 1, characterized in that: The protective gas in step 4 is argon, nitrogen or helium.
Citation Information
Patent Citations
Method for preparing orientation-reinforced Cu composite material for two-dimensional heat dissipation
CN103589894A
High-thermal-conductivity lamellar graphite / aluminum composite material and preparation method thereof
CN104707975A
Copper-based composite material cooling fin with graphite flakes arrayed in directional and layered manner and preparation method of copper-based composite material cooling fin
CN107116210A
Graphite, molybdenum and copper composite for electronic packaging and preparation method thereof
CN107955890A
Preparation method and application of crystalline flake graphite reinforced copper-based composite material
CN110343896A