A method for preparing natural rubber composite from recycled rubber powder of waste tire with controllable molecular weight

By using natural latex and ammonium bicarbonate solution to coordinate with inorganic metal salt, the molecular weight of waste tire powder is controlled, and the problems of low desulfurization efficiency and complex process in the existing technology are solved, and efficient and environmentally friendly waste tire regeneration is achieved. The preparation of rubber powder composite natural rubber materials has improved the mechanical properties and recycling value of the material.

CN118256029BActive Publication Date: 2024-11-22JULU COUNTY WANMEI RUBBER PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410393212.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-11-22
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

The prior art has low desulfurization efficiency, high energy consumption in the regeneration of waste tires, complex preparation process, contaminated by small-molecular solvents and regeneration reagents, and the impact of the molecular weight of the recycled rubber powder on the performance of composite rubber is not fully considered.

Method used

The natural latex and ammonium bicarbonate solution are used as green solvents, and the waste tire powder is fully penetrated and swelled by mechanical stirring and high-temperature heating. The coordinated action of inorganic metal salts and sulfur radicals is used to control the shear conditions to prepare regenerated glues of different molecular weights. Powder and mix with natural rubber to achieve the preparation of composite materials.

Benefits of technology

The preparation process is simplified, the molecular weight control accuracy of the recycled rubber powder is improved, the mechanical properties of the composite material are enhanced, and the high-value recycling of waste tire rubber powder is realized, and the process is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118256029B_ABST
    Figure CN118256029B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a composite natural rubber of waste tire recycled rubber powder with controllable molecular weight. The method is characterized in that natural latex and ammonium bicarbonate solution of a certain concentration are used as green solvents to fully penetrate and swell the waste tire rubber powder under mechanical stirring and high-temperature heating, so as to weaken the force between the molecular chains of the rubber powder and increase the plasticity; the treated waste tire rubber powder and inorganic metal salt are subjected to mechanical strong shearing in an internal mixer, and the sulfur free radicals generated by the rupture of the cross-linked network of the rubber powder can coordinate with the metal salt, on the one hand, preventing the free radicals from participating in the vulcanization cross-linking reaction again, and on the other hand, inhibiting the sulfur free radicals from attacking the unsaturated bonds of the main chain of the rubber powder molecule, and weakening the influence on the main chain structure of the rubber powder molecule during the regeneration process; the molecular weight of the waste tire recycled rubber powder is regulated by controlling the shearing temperature, rotation speed and shearing time; the obtained waste tire recycled rubber powder with different molecular weights is mixed with natural rubber and other additives on an open mixer to achieve good dispersion of the waste rubber powder, and hot pressing vulcanization is performed to prepare a composite material of waste tire recycled rubber powder and natural rubber, so as to exert the reinforcing effect of the waste rubber powder. The preparation process is simple, green and environmentally friendly, and is conducive to industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing composite natural rubber from waste tire recycled rubber powder with controllable molecular weight, and belongs to the field of waste rubber powder regeneration preparation. Background Art

[0002] With the continuous improvement of the automobile industry and manufacturing level, the number of waste tires is increasing. The main component of tires is vulcanized rubber, which is a thermosetting material. Abandoned tires cause serious black pollution problems. Therefore, it is urgent to treat waste tires through reasonable methods and realize recycling. However, before recycling, the desulfurization and regeneration problem of waste tires needs to be solved. At present, microwave desulfurization, radiation desulfurization, mechanical desulfurization, chemical regeneration agent desulfurization and other methods are mainly used to achieve the regeneration of waste tires. The essence of them is to destroy the cross-linking bonds of tires through energy, turning them into linear molecules, and improving the compatibility with other polymers and melt fluidity.

[0003] Zhang Shibo et al., China Plastics, 2023, 37(9):83-89, used cyclohexane oil as desulfurization solvent, 2,2′-dibenzamidodiphenyl disulfide and zinc oxide as catalysts to prepare low-temperature desulfurized rubber powder; Li Miao et al., Rubber and Plastic Technology and Equipment, 2015, 41(13):11-15, mixed the rubber powder and activator in a high-temperature stirred tank. The stirring temperatures were 140℃, 150℃, 160℃, and 170℃, respectively, and then the regeneration was carried out using a Haake torque rheometer, and the influence of the regeneration process was studied; Chinese patent CN202180069584.6 discloses a method for preparing styrene-butadiene rubber containing recycled rubber powder, wherein the rubber powder, water and surfactant are made into a suspension, and then mixed with a styrene-butadiene latex and flocculated to prepare a composite rubber; Si Hu et al., Polymer Materials Science and Engineering, 2012, 28(2):96-100, explored the effect of the activator on promoting desulfurization reaction and inhibiting crosslinking by adding an activator (alkylphenol polysulfide). The above preparation methods have low regeneration desulfurization efficiency, high energy consumption, and complex preparation process. If a higher desulfurization effect is to be achieved, the reaction temperature needs to be increased, and the use of small molecule solvents and regeneration agents generally has the problem of pollution and damage to the mechanical properties of rubber. At the same time, the molecular weight of the recycled rubber powder and the influence of the molecular weight on the properties of the composite rubber are not fully considered.

[0004] The invention uses environmentally friendly natural latex and ammonium bicarbonate solution as media, utilizes the coordination effect of inorganic metal salt and sulfur free radicals generated by the breakage of rubber powder to destroy the cross-linking network, controls the reaction conditions through mechanical shearing, and realizes the preparation of recycled rubber powder with different molecular weights. The preparation process is simple and green, and the invention is of great significance for the regeneration preparation and recycling of waste tire rubber powder. Summary of the invention

[0005] The invention aims to provide a method for preparing a composite natural rubber of waste tire recycled rubber powder with controllable molecular weight in view of the deficiencies of the prior art. The method is characterized in that natural latex and ammonium bicarbonate solution of a certain concentration are used as green solvents to fully penetrate and swell the waste tire rubber powder under mechanical stirring and high-temperature heating, so as to weaken the force between the molecular chains of the rubber powder and increase the plasticity; the treated waste tire rubber powder and inorganic metal salt are subjected to mechanical strong shearing in an internal mixer, and the sulfur free radicals generated by the rupture of the cross-linked network of the rubber powder under the action of shearing force can coordinate with the metal salt, on the one hand, preventing the sulfur free radicals from participating in the vulcanization cross-linking reaction again, and on the other hand, inhibiting the sulfur free radicals from attacking the unsaturated bonds of the main chain of the rubber powder molecules, so as to weaken the influence on the main chain structure of the rubber powder molecules during the regeneration process, and regulating the molecular weight of the waste tire recycled rubber powder by controlling the shearing temperature, the rotation speed and the shearing time; the obtained waste tire recycled rubber powder is mixed with natural rubber and other additives on an open mixer to achieve good dispersion of the waste rubber powder, and hot pressing vulcanization is performed to prepare a composite material of waste tire recycled rubber powder and natural rubber, so as to exert the reinforcing effect of the waste rubber powder.

[0006] The object of the present invention is achieved by the following technical scheme, wherein the raw material fractions are all mass fractions unless otherwise specified.

[0007] A method for preparing a composite natural rubber from recycled rubber powder of waste tires with controllable molecular weight, characterized in that the main raw materials are composed of the following components, calculated by mass:

[0008] 20-80 parts of waste tire rubber powder

[0009] Natural latex 100 parts

[0010] 75 parts of natural rubber

[0011] 5-15 parts of ammonium bicarbonate

[0012] 2-12 parts of inorganic metal salt

[0013] Wherein, the mesh size of the waste tire rubber powder is 30-100 mesh;

[0014] The inorganic metal salt is any one or two of zinc chloride, zinc acetate, zinc oxide, zinc sulfate, cupric chloride and ferric chloride.

[0015] The method for preparing the composite natural rubber from recycled rubber powder of waste tire with controllable molecular weight comprises the following steps:

[0016] Preparation of Controllable Molecular Weight Waste Tire Recycled Rubber Powder:

[0017] 100 parts of natural latex (solid content 25%) are diluted with deionized water to a concentration of 3-10wt%, 5-15 parts of ammonium bicarbonate are added and stirred until completely dissolved, then 20-80 parts of 30-100 mesh waste tire rubber powder are added, and the mixture is stirred and reacted at 80°C for 5-18 hours. The swelling effect of natural latex is combined with the expansion effect of the gas generated by the low-temperature decomposition of ammonium bicarbonate to make the rubber powder fully penetrate and swell, and the mixture is filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 2-12 parts of inorganic metal salt are subjected to mechanical strong shearing in an internal mixer, and the internal mixing temperature is 150-240°C, the internal mixing speed is 30-80 r / min, and the internal mixing time is 8-60 min. After the mixing, the mixture is naturally cooled to obtain waste tire recycled rubber powder with different molecular weights.

[0018] Preparation of natural rubber compounded with recycled rubber powder from waste tires:

[0019] The waste tire recycled rubber powder prepared above and 75 parts of natural rubber, 1-3 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 0.5-2 parts of sulfur are mixed evenly on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 140-180°C and 15 MPa for 8-40 min to obtain a natural rubber composite material.

[0020] The present invention has the following advantages:

[0021] The invention uses natural latex and ammonium bicarbonate solution as green and environmentally friendly solution media, fully swells waste tire rubber powder through natural latex, and utilizes ammonia and carbon dioxide generated by the decomposition of ammonium bicarbonate to penetrate the rubber powder, thereby increasing the distance between rubber molecular chains, weakening the entanglement of molecular chains, and increasing its plasticity, thereby promoting subsequent desulfurization and regeneration; polar sulfur free radicals have strong activity, and sulfur free radicals generated by the breakage of the rubber powder cross-linking network under mechanical shearing can coordinate with metal salts to prevent the re-crosslinking reaction after desulfurization, while weakening the influence on the main chain structure of the rubber powder molecule during the regeneration process, and by regulating the reaction conditions and processes of mechanical shearing temperature, rotation speed and time, recycled rubber powder with different molecular weights can be obtained. Through the mixing and processing of recycled rubber powder with different molecular weights and natural rubber, a natural rubber composite material with enhanced mechanical properties is prepared, thereby realizing the high-value recycling of waste tire rubber powder. The preparation method is simple, mild in conditions, highly efficient, and conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Scanning electron microscope image of the brittle fracture section of natural rubber composited with recycled rubber powder from waste tires

[0023] The recycled rubber powder from waste tires is well dispersed in the natural rubber matrix, with good interface bonding and no obvious phase separation. DETAILED DESCRIPTION

[0024] The present invention is further described below through specific examples. It should be noted that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make non-essential improvements and adjustments to the present invention based on the contents of the present invention described above. Example

[0025] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 10wt%, 4 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 20 parts of 50-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 6 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 4 parts of zinc chloride were subjected to mechanical strong shearing in an internal mixer, with an internal mixing temperature of 170°C, a internal mixing speed of 50 r / min, and an internal mixing time of 25 min. After the mixture was finished, it was naturally cooled to obtain waste tire recycled rubber powder. Using cyclohexane as solvent, the sol content was tested to be 58%, and xylene as mobile phase. The relative molecular weight of the recycled rubber powder sol was tested by gel permeation chromatography and was 93,000.

[0026] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 3 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.2 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 145°C and 15 MPa for 20 min to obtain a natural rubber composite material. The tensile strength was tested to be 6.4 MPa and the elongation at break was 479%. Example

[0027] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 8wt%, 5 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 30 parts of 80-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 6 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 6 parts of zinc oxide were subjected to mechanical strong shearing in a mixer, with a mixing temperature of 170°C, a mixing speed of 70 r / min, and a mixing time of 30 min. After the mixing, the mixture was naturally cooled to obtain waste tire recycled rubber powder. Using cyclohexane as the solvent, the sol content was tested to be 52%, and xylene as the mobile phase. The relative molecular weight of the recycled rubber powder sol was 84,000 as tested by gel permeation chromatography.

[0028] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 3 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 2 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 155°C and 15 MPa for 23 min to obtain a natural rubber composite material. The tensile strength was tested to be 6.9 MPa and the elongation at break was 424%. Example

[0029] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 6wt%, 6 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 35 parts of 100-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 8 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 8 parts of zinc acetate were subjected to mechanical strong shearing in a mixer, with a mixing temperature of 165°C, a mixing speed of 55 r / min, and a mixing time of 35 min. After the mixing, the waste tire recycled rubber powder was naturally cooled to obtain the recycled rubber powder. Using cyclohexane as the solvent, the sol content was tested to be 79%, and xylene as the mobile phase. The relative molecular weight of the recycled rubber powder sol was 119,000 according to gel permeation chromatography.

[0030] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 2 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.5 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 160°C and 15 MPa for 28 min to obtain a natural rubber composite material. The tensile strength was tested to be 10.1 MPa and the elongation at break was 527%. Example

[0031] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 6wt%, 6 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 35 parts of 100-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 8 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 8 parts of copper chloride were subjected to mechanical strong shearing in a mixer, with a mixing temperature of 165°C, a mixing speed of 55 r / min, and a mixing time of 35 min. After the mixing, the waste tire recycled rubber powder was naturally cooled to obtain the recycled rubber powder. Using cyclohexane as the solvent, the sol content was tested to be 72%, and xylene as the mobile phase. The relative molecular weight of the recycled rubber powder sol was 108,000 according to the gel permeation chromatography test with xylene as the mobile phase.

[0032] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 2 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.5 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 160°C and 15 MPa for 28 min to obtain a natural rubber composite material. The tensile strength was tested to be 9.2 MPa and the elongation at break was 548%. Example

[0033] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 6wt%, 6 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 35 parts of 100-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 8 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 8 parts of ferric chloride were subjected to mechanical strong shearing in a mixer, with a mixing temperature of 165°C, a mixing speed of 55 r / min, and a mixing time of 35 min. After the mixing, the waste tire recycled rubber powder was naturally cooled to obtain the recycled rubber powder. Using cyclohexane as the solvent, the sol content was tested to be 67%, and xylene was used as the mobile phase. The relative molecular weight of the recycled rubber powder sol was 101,000 according to the gel permeation chromatography test.

[0034] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 2 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.5 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 160°C and 15 MPa for 28 min to obtain a natural rubber composite material. The tensile strength was tested to be 9.5 MPa and the elongation at break was 488%. Example

[0035] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 3wt%, 12 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 80 parts of 60-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 15 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 4 parts of zinc chloride and 8 parts of zinc acetate were subjected to mechanical strong shearing in a mixer, with a mixing temperature of 190°C, a mixing speed of 60 r / min, and a mixing time of 40 min. After the mixing, the waste tire recycled rubber powder was naturally cooled to obtain the recycled rubber powder. Using cyclohexane as the solvent, the sol content was tested to be 64%, and xylene as the mobile phase. The relative molecular weight of the recycled rubber powder sol was 126,000 by gel permeation chromatography.

[0036] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 2 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.8 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 175°C and 15 MPa for 35 min to obtain a natural rubber composite material. The tensile strength was tested to be 13.8 MPa and the elongation at break was 579%. Example

[0037] 100 parts of natural latex (solid content 25%) were diluted with deionized water to a concentration of 3wt%, 12 parts of ammonium bicarbonate were added and stirred until completely dissolved, then 80 parts of 60-mesh waste tire rubber powder were added, and the mixture was stirred and reacted at 80°C for 15 hours to fully swell the rubber powder, and then filtered and vacuum dried at 60°C for 6 hours; the treated rubber powder and 4 parts of zinc oxide and 8 parts of cupric chloride were subjected to mechanical strong shearing in an internal mixer, with an internal mixing temperature of 190°C, an internal mixing speed of 60 r / min, and an internal mixing time of 40 min. After the mixture was finished, it was naturally cooled to obtain waste tire recycled rubber powder. Using cyclohexane as solvent, the sol content was tested to be 60%, and xylene as mobile phase. The relative molecular weight of the recycled rubber powder sol was 111,000 by gel permeation chromatography.

[0038] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 2 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.8 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 175°C and 15 MPa for 35 min to obtain a natural rubber composite material. The tensile strength was tested to be 13.2 MPa and the elongation at break was 601%.

[0039] Comparative Example 1

[0040] 20 parts of 50 mesh waste tire rubber powder were directly subjected to mechanical strong shearing in an internal mixer, with a mixing temperature of 170℃, a mixing speed of 50 r / min, and a mixing time of 25 min. After the mixing, the waste tire recycled rubber powder was naturally cooled. Using cyclohexane as the solvent, the sol content was tested to be 29%, and xylene as the mobile phase. The relative molecular weight of the recycled rubber powder sol was 64,000 according to gel permeation chromatography.

[0041] The waste tire recycled rubber powder prepared above was mixed evenly with 75 parts of natural rubber, 3 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 1.2 parts of sulfur on an open mill to achieve good dispersion of the waste rubber powder, and hot pressed at 145°C and 15 MPa for 20 min to obtain a natural rubber composite material. The tensile strength was tested to be 4.1 MPa and the elongation at break was 337%.

[0042] In summary, the embodiments of the present invention can obtain waste tire recycled rubber powder with controllable molecular weight by changing the concentration of natural latex, the content of ammonium bicarbonate, regulating the type and content of inorganic metal salts and the banburying shearing process. By mixing recycled rubber powders of different molecular weights with natural rubber, the mechanical properties of natural rubber are enhanced, thereby realizing the recycling of waste tire recycled rubber powder. Through Example 1 and Comparative Example 1, it can be seen that the waste tire rubber powder is activated by natural latex and ammonium bicarbonate and then reacted with metal salts, which can significantly improve the regeneration effect, increase the sol molecular weight, and improve the mechanical properties of the composite natural rubber.

[0043] The above embodiments describe the specific contents of the present invention in detail, but the present invention is not limited to the embodiments, and those skilled in the art can make equivalent substitutions, which should be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite natural rubber from recycled rubber powder of waste tires with controllable molecular weight, characterized in that: The main raw materials are composed of the following components, calculated by mass: 20-80 parts of waste tire rubber powder; 100 parts of natural rubber latex; 75 parts of natural rubber; 5-15 parts of ammonium bicarbonate; 2-12 parts of inorganic metal salt; The mesh size of the waste tire rubber powder is 30-100 mesh; the inorganic metal salt is any one or two of zinc chloride, zinc acetate, zinc oxide, zinc sulfate, copper chloride and ferric chloride; the preparation method of the controllable molecular weight waste tire recycled rubber powder composite natural rubber comprises the following steps: preparation of controllable molecular weight waste tire recycled rubber powder: dilute 100 parts of natural latex with a solid content of 25% with deionized water to a concentration of 3-10wt%, add 5-15 parts of ammonium bicarbonate and stir until completely dissolved, then add 20-80 parts of 30-100 mesh waste tire rubber powder, stir and react at 80°C for 5-18 h, utilize the swelling effect of natural latex combined with the expansion effect of the gas generated by the low-temperature decomposition of ammonium bicarbonate to make the rubber powder fully penetrate and swell, filter and vacuum dry at 60°C for 6 h; subject the treated rubber powder and 2-12 parts of inorganic metal salt to mechanical strong shear in an internal mixer, the internal mixing temperature is 150-240°C, the internal mixing speed is 30-80 r / min, and mixing time of 8-60 min. After the mixing, naturally cool the mixture to obtain waste tire recycled rubber powder with different molecular weights. Preparation of waste tire recycled rubber powder composite with natural rubber: Mix the prepared waste tire recycled rubber powder and 75 parts of natural rubber, 1-3 parts of zinc oxide, 0.5 parts of stearic acid, 0.5 parts of accelerator CZ, 0.3 parts of accelerator M, and 0.5-2 parts of sulfur on an open mixing mill to evenly mix them to achieve good dispersion of the waste rubber powder. Hot press at 140-180°C and 15 MPa for 8-40 min to obtain a natural rubber composite material.