A photocatalytic material and its preparation method and application
Nitrogen-doped copper phenylacetylene photocatalytic materials were prepared by hydrothermal method, which solved the problem of low catalytic oxidation efficiency of existing photocatalysts in water, achieved efficient removal of water pollutants, and demonstrated good reuse performance. .
Patent Information
- Application Number
- CN202410420312.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-09
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-04-09
AI Technical Summary
Existing photocatalysts have low catalytic oxidation efficiency when treating new pollutants in water bodies, and are difficult to reuse. In particular, the copper phenylacetylene material has insufficient oxidation ability and small surface area, which limits its photocatalytic activity.
A hydrothermal method was used to react Cu(OAc)2·H2O with raw materials such as L-histidine and phenylacetylene to prepare nitrogen-doped copper phenylacetylene (N/PPECu) photocatalytic material. By adjusting the molar ratio and reaction conditions, Enable efficient preparation and reuse of materials.
The specific surface area and oxidation ability of the photocatalyst are increased, which can effectively remove typical new pollutants in water, such as tetracycline antibiotics, and has good reuse performance and application potential.
Smart Images

Figure CN118268034B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalysts, and in particular relates to a photocatalytic material and a preparation method and application thereof. Background Art
[0002] In recent years, with the extensive use of antibiotics, hormones and anti-inflammatory drugs, the types and contents of new pollutants have continued to increase, which has seriously threatened the health and stability of natural water bodies. Therefore, it is urgent to improve the existing water treatment process to cope with the crisis brought about by drug pollution.
[0003] Photocatalysis is a technology that uses light energy to activate catalysts to promote chemical reactions. This technology has shown great application potential in the fields of environmental pollution control and energy conversion due to its environmentally friendly, efficient and sustainable characteristics. In terms of practical applications, photocatalysis has been applied in many fields such as water treatment, air purification, sterilization and deodorization. Especially in the field of water treatment, photocatalysis is considered to be one of the most valuable technologies due to its advantages such as simple operation, no secondary pollution and clean energy.
[0004] In the photocatalytic reaction, the semiconductor material acts as a catalyst, and the oxygen and water molecules adsorbed on its surface undergo charge separation under light conditions. - ) and valence band holes (h + ) migrate to different positions, electrons are adsorbed on the catalyst surface, while holes may react with water molecules to generate hydroxyl radicals (·OH). These ·OH have strong oxidizing ability and can effectively degrade organic pollutants. In order to improve the efficiency of photocatalysis, scientists modify and prepare new semiconductor materials through doping and composite methods; for example, by doping N, Sn, Si and other elements, the energy band structure of the semiconductor can be adjusted, thereby optimizing the separation efficiency of photogenerated carriers and reducing e - With h + The photocatalytic material is the key factor in determining the photocatalytic efficiency, and its performance will directly affect the efficiency of the entire process. However, the research in this field is not yet in-depth, for two reasons: 1. It is difficult to separate the powder material from the suspension and reuse it; 2. For sewage containing new pollutants, its catalytic oxidation efficiency is generally low and difficult to sustain.
[0005] Recently, a promising environmental remediation agent, phenylacetylene copper semiconductor photocatalyst, has attracted the interest of researchers due to its simple synthesis method, high response to visible light, and effective removal level in treating PPCPs pollution. However, the extremely negative CB position (about ~2.0V) and narrow Eg (~2.33eV) of PPECu lead to its weak oxidation ability, as well as low surface area and photogenerated e- -h + The rapid recombination of the pairs also severely limits their photocatalytic activity. At present, the application of metal-doped modified photocatalytic materials in water has made some progress, but the impact of non-metallic doping on their performance, the correlation between non-metallic doping and energy band regulation and its application value are still unclear.
[0006] Based on this, in order to solve the problem of residual typical new pollutants in environmental water bodies, the present invention provides a photocatalytic material to effectively remove typical new pollutants in water bodies. Summary of the invention
[0007] The purpose of the present invention is to provide a photocatalytic material and a preparation method and application thereof, which has the advantages of less raw materials, simple synthesis process and good repeatability, and can be used to overcome the shortcomings of using phenylacetylene copper as a photocatalyst to solve the problems existing in the above-mentioned prior art.
[0008] In order to achieve the above object, the present invention provides the following technical solutions:
[0009] A method for preparing a photocatalytic material comprises the following steps:
[0010] S1, Cu(OAc) 2 ·H 2 O is dissolved with a solvent, and then L-histidine is added and mixed evenly to obtain solution A;
[0011] S2, adding phenylacetylene and ascorbic acid to solution A, stirring and reacting at a first temperature for a first preset time, filtering, and drying and grinding the filter residue to obtain the photocatalytic material.
[0012] Preferably, in step S1, the solvent is methanol.
[0013] Preferably, in step S1, the Cu(OAc) 2 ·H 2 The molar ratio of O to L-histidine is 1:(0.5~1.25).
[0014] Preferably, in step S2, the Cu(OAc) 2 ·H 2 The molar ratio of O to phenylacetylene is 1:1.87.
[0015] Preferably, in step S2, the Cu(OAc) 2 ·H 2 The mass ratio of O to ascorbic acid is 1:1.25.
[0016] Preferably, in step S2, the first temperature is 70°C to 80°C.
[0017] Preferably, in step S2, the filter residue is washed three times with water and three times with ethanol respectively, then vacuum dried at 65° C. for 8 h, and then ground to obtain the photocatalytic material.
[0018] The present invention also provides a photocatalytic material, which is prepared by any of the above preparation methods.
[0019] The present invention also provides the use of the above-mentioned photocatalytic material as a photocatalyst in degrading water pollutants.
[0020] Preferably, the water pollutant is a tetracycline antibiotic.
[0021] Beneficial effects:
[0022] (1) The present invention adopts a hydrothermal method to achieve the regulation of xN / PPECu photocatalytic materials and to prepare N-doped phenylacetylene copper (N / PPECu) using L-histidine as a nitrogen element supplier. It has the advantages of less raw materials, simple synthesis process and good repeatability, and also has the basic conditions for large-scale production, as well as high application potential and use value;
[0023] (2) The photocatalytic material provided by the present invention is a nitrogen-doped copper phenylacetylene composite photocatalytic material, which can efficiently remove typical new pollutants in water bodies and is an environmentally friendly photocatalyst with energy-saving effects. It can be used to overcome the shortcomings of using copper phenylacetylene as a photocatalyst, which is beneficial to solving the technical defects of difficult treatment of trace pollutants in water bodies, and can effectively degrade pollutants in water bodies under light. In addition, the photocatalytic material of the present application has the excellent performance of being easy to recycle and reuse. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. Among them:
[0025] Figure 1 XRD diagrams of the xN / PPECu composite photocatalytic materials of Examples 1, 2, 3, and 4 of the present application and the PPECu photocatalyst of Comparative Example 1;
[0026] Figure 2 The photocatalytic activity diagram of tetracycline (TC) reduction based on different nitrogen doping ratios of the xN / PPECu composite photocatalytic materials of Examples 1, 2, 3 and 4 of the present application and the PPECu photocatalyst of Comparative Example 1 under visible light irradiation;
[0027] Figure 3The SEM and TEM images of the 0.75N / PPECu composite photocatalytic material of Example 2 of the present application and the PPECu photocatalyst of Comparative Example 1;
[0028] Figure 4 It is a transient photocurrent response diagram of the 0.75N / PPECu composite photocatalytic material of Example 2 of the present application and the PPECu photocatalyst of Comparative Example 1;
[0029] Figure 5 The ultraviolet diffuse reflectance spectra of the 0.75N / PPECu composite photocatalytic material prepared in Example 2 of the present application and the PPECu photocatalyst of Comparative Example 1;
[0030] Figure 6 The band gap energy diagram of the 0.75N / PPECu composite photocatalytic material prepared in Example 2 of the present application and the PPECu photocatalyst of Comparative Example 1;
[0031] Figure 7 This is a degradation kinetic diagram of tetracycline (TC) by the 0.75N / PPECu composite photocatalytic material of Example 2 of the present application in a natural water sample for 5 minutes;
[0032] Figure 8 This is a tetracycline (TC) degradation kinetics diagram measured when the 0.75N / PPECu composite photocatalytic material of Example 2 of the present application was used continuously for 20 minutes and recycled every 5 minutes. DETAILED DESCRIPTION
[0033] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0034] The present invention will be described in detail below in conjunction with embodiments. It should be noted that the embodiments and features in the embodiments of the present invention can be combined with each other without conflict.
[0035] In view of the problems existing in current photocatalysts, the present invention provides a method for preparing a photocatalytic material, comprising the following steps:
[0036] S1, Cu(OAc) 2 ·H 2 O is dissolved with a solvent, and then L-histidine is added and mixed evenly to obtain solution A;
[0037] S2, adding phenylacetylene and ascorbic acid to solution A, stirring and reacting at a first temperature for a first preset time, filtering, and drying and grinding the filter residue to obtain a photocatalytic material.
[0038] The photocatalytic material prepared by the method is essentially a nitrogen-doped phenylacetylene copper photocatalytic material, which is named N / PPECu or xN / PPECu in the present invention, wherein "x" refers to the N / Cu ratio.
[0039] In a preferred embodiment of the present invention, in step S1, the solvent is methanol.
[0040] In a preferred embodiment of the present invention, in step S1, Cu(OAc) 2 ·H 2 The molar ratio of O to L-histidine is 1:(0.5~1.25) to obtain N / PPECu photocatalytic materials with a N / Cu ratio of 0.5~1.25 (e.g., 0.5, 0.75, 1.0, 1.25).
[0041] In a preferred embodiment of the present invention, in step S2, Cu(OAc) 2 ·H 2 The molar ratio of O to phenylacetylene is 1:1.87.
[0042] In a preferred embodiment of the present invention, in step S2, Cu(OAc) 2 ·H 2 The mass ratio of O to ascorbic acid is 1:1.25.
[0043] In a preferred embodiment of the present invention, in step S2, the first temperature is 70°C to 80°C (eg, 70°C, 75°C, 80°C).
[0044] In a preferred embodiment of the present invention, in step S2, the filter residue is washed three times with water and three times with ethanol respectively, then vacuum dried at 65° C. for 8 h, and then ground to obtain the photocatalytic material.
[0045] The present invention also provides a photocatalytic material, which is prepared by any of the above preparation methods.
[0046] The present invention also provides the use of the above-mentioned photocatalytic material as a photocatalyst in degrading water pollutants.
[0047] In a preferred embodiment of the present invention, the water pollutant is a tetracycline antibiotic.
[0048] The photocatalytic material of the present invention and its preparation method and application are described in detail below through specific embodiments.
[0049] Example 1
[0050] This embodiment provides a N / PPECu photocatalytic material, and the preparation steps are as follows:
[0051] Weigh 0.200g of Cu(OAc) 2·H 2 O powder was fully dispersed in 40 mL of methanol, 0.755 g of L-histidine (His) was added, and the mixture was vigorously stirred for 1 hour using a stirrer to obtain solution A. After the reaction was completed, 0.205 mL of phenylacetylene and 0.250 g of ascorbic acid were added to solution A, and the mixture was heated and stirred at 75°C for 30 minutes using a stirrer to obtain a yellowish green sample. The sample was placed in an oven, dried overnight at 60°C, and then ground into powder using an agate mortar for use, thereby obtaining a xN / PPECu composite photocatalytic material with a molar ratio of N / Cu=0.5.
[0052] Example 2
[0053] This embodiment provides a N / PPECu photocatalytic material, and the preparation steps are as follows:
[0054] Weigh 0.200g of Cu(OAc) 2 ·H 2 O powder was fully dispersed in 40 mL of methanol, 1.162 g of L-histidine (His) was added, and the mixture was vigorously stirred for 1 hour using a stirrer to obtain solution A. After the reaction was completed, 0.205 mL of phenylacetylene and 0.250 g of ascorbic acid were added to solution A, and the mixture was heated and stirred at 75°C for 30 minutes using a stirrer to obtain a yellowish green sample. The sample was placed in an oven, dried overnight at 60°C, and then ground into powder using an agate mortar for use, thereby obtaining a xN / PPECu composite photocatalytic material with a molar ratio of N / Cu=0.75.
[0055] Example 3
[0056] This embodiment provides a N / PPECu photocatalytic material, and the preparation steps are as follows:
[0057] Weigh 0.200g of Cu(OAc) 2 ·H 2 O powder was fully dispersed in 40 mL of methanol, 1.550 g of L-histidine (His) was added, and the mixture was vigorously stirred for 1 hour using a stirrer to obtain solution A. After the reaction was completed, 0.205 mL of phenylacetylene and 0.250 g of ascorbic acid were added to solution A, and the mixture was heated and stirred at 75°C for 30 minutes using a stirrer to obtain a yellowish green sample. The sample was placed in an oven, dried overnight at 60°C, and ground into powder using an agate mortar for use, thereby obtaining a xN / PPECu composite photocatalytic material with a molar ratio of N / Cu=1.
[0058] Example 4
[0059] This embodiment provides a N / PPECu photocatalytic material, and the preparation steps are as follows:
[0060] Weigh 0.200g of Cu(OAc) 2 ·H 2 O powder was fully dispersed in 40 mL of methanol, 1.938 g of L-histidine (His) was added, and the mixture was vigorously stirred for 1 hour using a stirrer to obtain solution A. After the reaction was completed, 0.205 mL of phenylacetylene and 0.250 g of ascorbic acid were added to solution A, and the mixture was heated and stirred at 75°C for 30 minutes using a stirrer to obtain a yellowish green sample. The sample was placed in an oven, dried overnight at 60°C, and then ground into powder using an agate mortar for use, thereby obtaining a xN / PPECu composite photocatalytic material with a molar ratio of N / Cu=1.25.
[0061] Comparative Example 1
[0062] This comparative example is the preparation of phenylacetylene copper (PPECu), and the specific steps are as follows:
[0063] Weigh 0.200g of Cu(OAc) 2 ·H 2 O powder was fully dispersed in 40 mL of methanol, 0.205 mL of phenylacetylene and 0.250 g of ascorbic acid were added, and the mixture was heated and stirred at 75 °C with a stirrer for 30 min to obtain a bright yellow powder, which was transferred to a centrifuge tube and washed three times with pure water and ethanol by centrifugation in a centrifuge, and then placed in a vacuum drying oven at 65 °C for 8 h to obtain a PPECu photocatalyst.
[0064] Characterization:
[0065] The crystal and phase structures of Examples 1, 2, 3, 4 and Comparative Example 1 were studied by X-ray diffraction. Figure 1 As shown in the figure, the XRD patterns of PPECu samples with different nitrogen doping ratios have similar characteristics, but there are also obvious differences. When N is introduced, the (100) and (001) of N / PPECu weaken and broaden, which also shows that the periodic stacking of xN / PPECu becomes less compact and disordered. The decrease in the (101) peak means that the growth mode of nitrogen-modified phenylacetylene copper has changed. This change makes the photocatalyst have a larger specific surface area, which is consistent with the nitrogen adsorption-desorption results. In addition, the introduction of N prevents phenylacetylene copper from developing towards larger and more elongated crystals.
[0066] Photocatalytic activity test:
[0067] In the visible light (9 W blue light emitting diode LED light, wavelength 455-460 nm, illumination 6.6 mW / cm 2 ) irradiation, the photocatalytic degradation activity of tetracycline antibiotics in Examples 1, 2, 3, 4 and Comparative Example 1 was evaluated. Figure 2As shown in the figure, under blue light irradiation, nitrogen-doped copper phenylacetylene showed superior photocatalytic ability than PPECu, achieving a degradation rate of tetracycline (20 mg / L) of >95% within 5 minutes. Among them, the successful introduction of the N element expanded the specific surface area of the photocatalyst and provided more reactive sites, which made xN / PPECu have a higher adsorption performance for TC in the experiment, and the high adsorption rate also means that the kinetic performance of tetracycline degradation in the system can be improved. Obviously, 0.75N / PPECu has the highest photocatalytic activity, and its kinetic rate constant is about 5.54 times that of PPECu. Therefore, subsequent experiments are all based on copper phenylacetylene with N / Cu of 0.75 as the research object to further study the mechanism of 0.75N / PPECu photodegradation of TC.
[0068] TEM characterization:
[0069] The 0.75N / PPECu composite photocatalytic material of Example 2 and the PPECu photocatalyst of Comparative Example 1 were characterized by SEM and TEM. Figure 3 As shown in the SEM and TEM images, PPECu has a smooth nanowire structure. After modification with histidine, the morphology of PPECu changes significantly. The nanowire structure of 0.75N / PPECu is transformed into a shorter granular structure like rice grains. On the one hand, these granular structures can expand their specific surface area, which is conducive to the adsorption of organic pollutants. On the other hand, due to the increase in the reaction sites of the photocatalyst, the photocatalytic degradation of tetracycline (TC) is also enhanced.
[0070] Electrochemical performance test:
[0071] The electrochemical performance of the 0.75N / PPECu composite photocatalytic material of Example 2 and the PPECu photocatalyst of Comparative Example 1 was tested using an electrochemical workstation. Figure 4 The transient photocurrent response diagram of PPECu photocatalyst and 0.75N / PPECu composite photocatalyst is measured. The main test is the light response ability of PPECu photocatalyst and 0.75N / PPECu composite photocatalyst at the moment of starting light (light on) and turning off light (light off). It can be seen that compared with PPECu photocatalyst, 0.75N / PPECu composite photocatalyst shows stronger photocurrent and good photoelectric stability, showing that nitrogen doping is beneficial to inhibiting photogenerated carrier recombination.
[0072] UV diffuse reflectance spectrum test:
[0073] The 0.75N / PPECu composite photocatalytic material of Example 2 and the PPECu photocatalyst of Comparative Example 1 were tested by ultraviolet diffuse reflectance spectroscopy. The results are as follows: Figure 5 and Figure 6 shown. Figure 5 The UV diffuse reflectance spectra of the 0.75N / PPECu composite photocatalytic material prepared in Example 2 of the present application and the PPECu photocatalyst of Comparative Example 1 are shown. Figure 5 It can be seen that compared with PPECu (522nm), the absorption edge of 0.75N / PPECu is slightly red-shifted to 528nm, which means that 0.75N / PPECu has stronger light absorption ability, which is beneficial to improving the photodegradation efficiency of TC. Therefore, the composite photocatalytic material has stronger potential for photocatalytic reaction.
[0074] Figure 6 The band gap energy (Eg) diagram of the photocatalyst was calculated according to the Kubelka-Munk formula, and the band gap energy of the PPECu photocatalyst was obtained to be 2.456eV, while that of 0.75N / PPECu was 2.484eV, which shows that the 0.75N / PPECu composite photocatalytic material has an excellent ability to utilize light energy, proving the feasibility of the application of the 0.75N / PPECu composite photocatalytic material.
[0075] Application Example 1
[0076] The 0.75N / PPECu composite photocatalytic material prepared in Example 2 is used to treat TC in natural wastewater, and the specific steps are as follows:
[0077] (1) Take actual water bodies such as tap water, Pearl River water and seawater, add 50 mL of the drug tetracycline (TC) to make the concentration of tetracycline (TC) in the actual water be 20 mg / L, add 10 mg of the composite photocatalytic material, and stir in the dark for 30 minutes to achieve adsorption / dissociation equilibrium. During this process, ultrapure water is taken as the control group;
[0078] (2) Then, visible light (9W blue light emitting diode LED lamp, wavelength 455-460nm, illumination 6.6mW / cm2) was used for photocatalytic reaction. At a specific time interval, 1mL of the reaction solution was taken and filtered through a 0.45μm microporous filter. The reaction solution was then used for liquid chromatography to detect the pollutant content, which was recorded as C. According to the formula N = (C 0 -C)×100% to calculate the TC removal rate N, where C 0 is the initial concentration of TC.
[0079] Figure 7 The degradation kinetics of TC by the 0.75N / PPECu composite photocatalytic material prepared in Example 2 in natural water samples for 5 min is shown in FIG. Figure 7It can be seen that the N / PPECu composite photocatalytic material has a good photocatalytic degradation effect on TC, whether in ultrapure water (described as Ultrapure water in the figure) or in other natural water bodies.
[0080] Application Example 2
[0081] This application example uses the 0.75N / PPECu composite photocatalytic material prepared in Example 2 to treat tetracycline (TC) in actual water, and the reusability of the 0.75N / PPECu composite photocatalytic material is tested. The specific steps are as follows:
[0082] (1) Add tetracycline (TC) to ultrapure water to prepare a 50 ml tetracycline (TC) solution and place it in a beaker so that the concentration of tetracycline (TC) in the solution is 20 mg / L. Then take 10 mg of the composite photocatalytic material and add it to the beaker for adsorption in the dark for 30 minutes.
[0083] (2) Then use visible light (9W blue light emitting diode LED light, wavelength 455-460nm, illumination 6.6mW / cm 2 ) irradiation for photocatalytic reaction, the total reaction time is 20 min, at specific time intervals, 1 mL of the reaction solution is taken and filtered through a 0.45 μm microporous filter, the concentration of the remaining tetracycline (TC) in the solution is determined by liquid chromatography, the 0.75N / PPECu composite photocatalytic material reacted in the above tetracycline (TC) solution is taken out every 5 min, and a suction filter is used to filter while washing with ultrapure water and ethanol, the washed 0.75N / PPECu composite photocatalytic material is dried in an oven at 60°C overnight, and the 0.75N / PPECu composite photocatalytic material is removed from the filter paper and ground again, and then continued to be added to the above tetracycline (TC) solution for photocatalytic degradation reaction, the total reaction time is 20 min, and samples are taken at specific time points within 20 min. Except for the different batches of photocatalyst used in each cycle experiment, the other conditions are the same.
[0084] The results are as follows Figure 8 As shown, Figure 8 This is a kinetic diagram of tetracycline (TC) degradation when the 0.75N / PPECu composite photocatalytic material of Example 2 of the present application is used continuously for 20 minutes and recycled every 5 minutes. Figure 8It can be seen that the photocatalytic removal rate of tetracycline (TC) degrading in water bodies after four repeated applications of the 0.75N / PPECu composite photocatalytic material within 20 minutes remained above 80%, indicating that the 0.75N / PPECu composite photocatalytic material in this application still has high photocatalytic performance after repeated use for 4 times. The 0.75N / PPECu composite photocatalytic material exhibits good reuse performance and application potential for degrading tetracycline (TC) in aqueous solutions.
[0085] In summary:
[0086] The present invention doped nitrogen on the PPECu photocatalyst with high photocatalytic activity, successfully prepared N-doped phenylacetylene copper (N / PPECu), and obtained the optimal nitrogen doping ratio after adjustment. The present invention also provides the application of the xN / PPECu composite photocatalytic material under blue light LED illumination to achieve efficient degradation of tetracycline (TC). The present invention applies the 0.75N / PPECu composite photocatalytic material to actual natural water conditions to treat tetracycline (TC), an antibiotic pollutant. At the same time, the present invention provides a new idea for the element doping modification strategy of phenylacetylene copper, and also provides a reference for the development of green photocatalysis and efficient wastewater purification technology. Therefore, it has broad application prospects in sewage treatment, water body reduction, adsorption degradation and other aspects.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a photocatalytic material, characterized in that: The steps include: S1, dissolving Cu(OAc)2·H2O with a solvent, then adding L-histidine and mixing evenly, wherein the molar ratio of Cu(OAc)2·H2O to L-histidine is 1:(0.5-1.25), to obtain solution A; S2. Add phenylacetylene and ascorbic acid to solution A, wherein the molar ratio of Cu(OAc)2·H2O to phenylacetylene is 1:1.87, and the mass ratio of Cu(OAc)2·H2O to ascorbic acid is 1:1.
25. Stir the reaction at a first temperature for a first preset time, filter, dry and grind the filter residue to obtain the photocatalytic material.
2. The method for preparing a photocatalytic material according to claim 1, characterized in that: In step S1, the solvent is methanol.
3. The method for preparing a photocatalytic material according to claim 1, characterized in that: In step S2, the first temperature is 70°C to 80°C.
4. The method for preparing a photocatalytic material according to claim 1, characterized in that: In step S2, the filter residue is washed three times with water and three times with ethanol respectively, then vacuum dried at 65° C. for 8 h, and then ground to obtain the photocatalytic material.
5. A photocatalytic material, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 4.
6. Use of the photocatalytic material as claimed in claim 5 as a photocatalyst in degrading water pollutants.
7. The use according to claim 6, characterized in that The water pollutant is tetracycline antibiotics.