A quaternary ammonium salt polysulfone containing different side chain lengths and its preparation method and application
By introducing quaternary ammonium salt groups of different side chain lengths into the polysulfone, the problem of single side chain length of quaternary ammonium polysulfone in the prior art is solved, and the regulation of its hydrophilicity, lipophilicity and antibacteriality is achieved. , improving its functional performance.
Patent Information
- Application Number
- CN202410376313.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-29
AI Technical Summary
The quaternary ammonium polysulfone prepared in the prior art has a single side chain length and cannot effectively regulate its hydrophilicity, lipophilicity and solubility, limiting the application and development of its functional materials.
After chloromethylation of the polysulfone, quaternary ammonium salt groups of different side chain lengths are introduced to control the degree of substitution of chloromethylation and the side chain length of the quaternary ammonium salt, and the hydrophilicity and antibacterial properties of the polysulfone are regulated. , realize the comprehensive performance optimization of quaternary ammonium polysulfone.
The versatility improvement of quaternary ammonium polysulfone is achieved, including solubility and antibacterial effects in water and ethanol, enhancing its performance in different environments.
Smart Images

Figure CN118271616B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of quaternary ammonium salt materials, in particular to a quaternary ammonium salt polysulfone containing different side chain lengths and a preparation method and application thereof. Background Art
[0002] Quaternary ammonium salts are an important class of cationic surfactants and also a commonly used class of organic antibacterial agents. Their antibacterial mechanism is relatively complex, but it is generally believed that their action process is as follows: Quaternary ammonium salt cationic antibacterial agents carry a positive charge, while the phosphate groups on the surface of microbial cells are electronegative. Through electrostatic adsorption, quaternary ammonium salt cationic antibacterial agents can destroy the cell membrane of microorganisms and enter the body of microorganisms, denaturing proteins and inactivating enzymes, causing the leakage of active substances in the microorganisms (such as potassium salts, ribonucleic acid, etc.), leading to cell disintegration and death.
[0003] Polysulfone is a kind of high performance engineering plastic, is famous for its excellent high thermal stability and chemical stability and high mechanical strength, and these excellent performances make it be widely used in multiple industries, comprise medical and industrial membrane technology, fuel cell assembly, water treatment process, biomedical equipment, gas separation system and composite material development.In order to further improve the performance of polysulfone and expand its range of application, it is carried out quaternization modification, makes polysulfone have multiple functions such as anion exchange capacity, strong hydrophilicity and antibiotic property, therefore, receives extensive attention of those skilled in the art.But the quaternary ammonium salt polysulfone prepared by prior art is mainly the quaternary ammonium salt functional group of single side chain length, cannot realize its comprehensive performance is regulated and controlled, and then limits the further application and development of quaternary ammonium salt polysulfone functional material.
[0004] In order to solve the above-mentioned technical problems, the inventors in the previous work (patent publication number is CN112876682A), the present invention considers that polysulfone is a kind of thermoplastic engineering plastics, has good mechanical strength and chemical stability, therefore with polysulfone as raw material, by chloromethylating polysulfone, then react with trimethylamine aqueous solution, to generate water-soluble quaternary ammonium salt polysulfone. Although this method can improve the hydrophilicity and antibacterial property of polysulfone material to a certain extent, it is impossible to achieve defects such as regulating and controlling its hydrophilicity, lipophilicity and solubility in solvents such as ethanol.
[0005] To this end, the present invention provides a quaternary ammonium salt polysulfone containing different side chain lengths and a preparation method and application thereof. Summary of the invention
[0006] In order to solve the above-mentioned deficiencies in the prior art, the present invention provides a quaternary ammonium salt polysulfone containing different side chain lengths and a preparation method and application thereof. The present invention chloromethylates the polysulfone and then introduces a quaternary ammonium salt group with a corresponding side chain length according to demand, so as to improve the hydrophilicity and antibacterial property of the polysulfone by controlling the chloromethyl substitution degree of the chloromethylation and the side chain length of the quaternary ammonium salt, thereby enabling the quaternary ammonium salt polysulfone prepared by the present invention to be used as an antibacterial agent material.
[0007] The quaternary ammonium salt polysulfone containing different side chain lengths and the preparation method and application thereof of the present invention are achieved by the following technical scheme:
[0008] The first object of the present invention is to provide a method for preparing quaternary ammonium salt polysulfone containing different side chain lengths. The present invention takes into account that the carbon chain length in quaternary ammonium salt has a certain influence on the antibacterial property of quaternary ammonium salt, and is mainly manifested in the following aspects: 1) carbon chain length and fat solubility. The longer the carbon chain of quaternary ammonium salt is, the stronger its fat solubility is, which makes them easier to penetrate the cell membrane of bacteria, thereby enhancing its antibacterial effect; 2) carbon chain length and surface activity. Quaternary ammonium salt is a surfactant. The increase of its carbon chain length can enhance its surface activity, help to reduce the tension on the surface of bacterial cells, and then destroy the cell membrane; 3) carbon chain length and selectivity. Generally speaking, the increase of carbon chain length can improve the selectivity to gram-positive bacteria; but if the carbon chain is too long, its water solubility may be reduced, thereby affecting its use effect in an aqueous environment; 4) optimal carbon chain length: studies have shown that when the carbon chain length in the quaternary ammonium salt molecule is within a certain range, its antibacterial effect is the best, and beyond this range, the antibacterial effect may decline. In a word, the length of the carbon chain in the quaternary ammonium salt has a significant influence on its antibacterial property. Therefore, the present invention proposes to introduce groups with different carbon chain lengths into the quaternary ammonium salt, so as to achieve the regulation of the comprehensive properties of the quaternary ammonium salt polysulfone by regulating the carbon chain length of the introduced group, and the preparation method of the present invention comprises the following steps:
[0009] Step 1, preparation of chloromethylated polysulfone:
[0010] The polysulfone is subjected to chloromethylation treatment to obtain chloromethylated polysulfone.
[0011] It should be emphasized that, in the present invention, the polysulfone is first subjected to chloromethylation treatment, so as to achieve the chloromethylation modification treatment of the polysulfone molecule by introducing chloromethyl groups into the polysulfone molecule.
[0012] It should be noted that when the polysulfone is subjected to chloromethylation treatment in the present invention, the chloromethylation degree of substitution of the polysulfone should not be too small, otherwise the number of quaternary ammonium salt functional groups introduced will be too small; the chloromethylation degree of substitution should not be too large, otherwise crosslinking will occur during the preparation of chloromethyl polysulfone. Therefore, in a preferred embodiment of the present invention, the chloromethylation degree of substitution is in the range of 1.0 to 1.6.
[0013] In order to ensure that the chloromethylated polysulfone with a chloromethylation degree of substitution in the range of 1.0 to 1.6 can be obtained, in a preferred embodiment of the present invention, the chloromethylated polysulfone is prepared by the following steps:
[0014] The polysulfone, paraformaldehyde, trimethylsilyl chloride and a catalyst are dissolved in a solvent, and heated at 45-55° C. under the protection of nitrogen or an inert gas until the chloromethylation substitution degree is within the range of 1.0-1.6 to obtain the chloromethylated polysulfone.
[0015] It should be noted that, in the preparation of chloromethylated polysulfone, chlorohydrocarbon is used as solvent, polysulfone, paraformaldehyde and trimethylchlorosilane are used as raw materials, and anhydrous tin tetrachloride is used as catalyst. During the heating reaction under the protection of nitrogen or inert gas, chloromethylation reaction occurs to obtain chloromethylated polysulfone. The reaction liquid in the heating process is collected, purified and then subjected to nuclear magnetic resonance detection, and the chloromethyl substitution degree of the polysulfone at different reaction times is monitored by nuclear magnetic resonance.
[0016] In order to separate and purify chloromethylated polysulfone, the present invention cools the reaction liquid after the heating reaction to room temperature, slowly pours the cooled reaction liquid into ethanol precooled to 0°C at a stirring rate of 300-350 r / min for precipitation, collects the obtained precipitate, dissolves it with chloroform, precipitates it with ethanol, repeats it 3 times, filters it, and washes it with ethanol at least 3 times to remove excess paraformaldehyde, trimethylsilyl chloride and catalyst tin tetrachloride. Then, the washed precipitate is vacuum dried at 50°C for 12-24 hours to obtain solid chloromethylated polysulfone.
[0017] In a preferred embodiment of the present invention, when preparing chloromethylated polysulfone, the amount ratio of polysulfone, paraformaldehyde, trimethylsilyl chloride, catalyst and solvent used is 10g:8-10g:50-60mL:0.5-1.0mL:500-800mL.
[0018] In a preferred embodiment of the present invention, the present invention takes into account that the chloromethylation reaction follows an electrophilic substitution mechanism and needs to use a chlorinated hydrocarbon as a solvent, so the solvent used in the present invention can be selected from any one of chloroform, dichloroethane and trichloroethane. Among them, considering the preparation cost, chloroform is selected as the solvent when preparing highly substituted chloromethyl polysulfone. In the preparation of low-substituted chloromethyl polysulfone, dichloromethane can be used as the solvent.
[0019] Step 2, dissolving the chloromethylated polysulfone in a solvent, adding a tertiary amine compound A containing a carbon straight-chain alkyl group with a carbon number of ≥6 under the protection of an inert gas, mixing, and performing a quaternization reaction to introduce an R2 group on the chloromethylated polysulfone to obtain an intermediate product; adding a tertiary amine compound B containing a carbon straight-chain alkyl group with a carbon number of 1 to 4 to the intermediate product, and performing a quaternization reaction to introduce an R1 group on the intermediate product, that is, obtaining a quaternary ammonium salt polysulfone having both an R2 group and an R1 group as shown in formula I;
[0020]
[0021] It should be emphasized that, in order to regulate the comprehensive properties of quaternary ammonium salt polysulfone, the present invention first introduces R2 group into chloromethylated polysulfone, and R2 group is a carbon straight chain alkyl with carbon number ≥ 6, so as to improve the lipophilicity and compatibility of other plastics of polysulfone by introducing R2 group. Then, on the basis of the intermediate product obtained after the introduction of R2 group, R1 group is further introduced, and R1 group is a carbon straight chain alkyl with carbon number 1 to 5, so as to improve the hydrophilicity and other properties of polysulfone by further introducing R1 group, so as to realize the improvement of the comprehensive properties of quaternary ammonium salt polysulfone by the combined action of the introduced R2 group and R1 group.
[0022] In order to realize the introduction of R2 group on chloromethylated polysulfone, the present invention preferably uses tertiary amine compound A having R2 group as a precursor for introducing R2 quaternary ammonium salt group, and tertiary amine compound A is subjected to quaternization reaction with chloromethyl group in chloromethylated polysulfone to realize the introduction of R2 group on chloromethylated polysulfone. And in order to ensure that R2 group can be introduced on chloromethylated polysulfone through tertiary amine compound A, in a preferred embodiment of the present invention, tertiary amine compound A is any one of N,N-dimethyl n-hexylamine, N,N-dimethyl n-octylamine, N,N-dimethyl n-heptylamine and N,N-dimethyl tertiary amine with more than 8 carbon straight-chain alkyl groups. In another preferred embodiment of the present invention, the R2 group is a carbon straight-chain alkyl group with 6 to 8 carbon atoms; that is, the corresponding tertiary amine compound A used is any one of N,N-dimethyl n-hexylamine, N,N-dimethyl n-octylamine and N,N-dimethyl n-heptylamine.
[0023] In order to realize the chloromethylated polysulfone after the R2 group has been introduced, that is, the R1 group is further introduced on the basis of the intermediate product, preferably, a tertiary amine compound B having the R1 group is used as a precursor for introducing the R1 quaternary ammonium salt group, and the tertiary amine compound B is allowed to continue to react with the remaining chloromethyl groups in the chloromethylated polysulfone to carry out a quaternization reaction, so as to further introduce the R1 group on the basis of the intermediate product, thereby obtaining a quaternary ammonium salt polysulfone having both the R2 group and the R1 group. In order to ensure that the R1 group can be introduced into the chloromethylated polysulfone through the tertiary amine compound B, in a preferred embodiment of the present invention, the tertiary amine compound B is any one of trimethylamine, N,N-dimethylethylamine, N,N-dimethyl-n-propylamine, N,N-dimethyl-n-butylamine and N-methyl-n-pentylamine. In another preferred embodiment of the present invention, the R1 group is a straight-chain alkyl group having 1 to 4 carbon atoms; that is, the corresponding tertiary amine compound B used is any one of trimethylamine, N,N-dimethylethylamine, N,N-dimethyl-n-propylamine and N,N-dimethyl-n-butylamine.
[0024] In order to facilitate the introduction of R2 groups in chloromethylated polysulfone in a solution state, in a preferred embodiment of the present invention, the solvent used to dissolve the chloromethylated polysulfone is any one of DMF, DMSO and NMP, and the mass ratio of the tertiary amine compound A to the above solvent is 1:20-30, so as to ensure that the tertiary amine compound A can be fully dissolved in the solvent, so as to facilitate the introduction of the R2 quaternary ammonium salt group in the subsequent reaction process. In another preferred embodiment of the present invention, considering that the boiling point of DMF is relatively low, it is easy to remove by vacuum distillation, and the high-boiling tertiary amine can also be taken out at the same time, so DMF is preferably used as a solvent for dissolving chloromethylated polysulfone.
[0025] It should also be noted that the reaction temperature for the quaternization reaction after adding the tertiary amine compound A is selected according to the specific tertiary amine compound actually selected, and the selected temperature should meet the requirements of accelerating the reaction while minimizing the volatilization of the tertiary amine. For example, when the tertiary amine compound A is N,N-dimethyl-n-hexylamine, N,N-dimethyl-n-octylamine and other high-boiling amines (N,N-dimethyl tertiary amines with more than 8 carbon straight-chain alkyl groups), the reaction temperature is 90-100°C and the reaction time is 8-24h.
[0026] In order to facilitate the further introduction of the R1 group by the tertiary amine compound B in a solution state on the basis of the already introduced R2 group, in a preferred embodiment of the present invention, the molar ratio of the tertiary amine compound A to the tertiary amine compound B is 1:2-8, and the molar ratio of the total molar amount of the tertiary amine compound A and the tertiary amine compound B to the chloromethylated polysulfone is 3-4:1, so as to ensure that after the tertiary amine compound A is added to react with the chloromethylated polysulfone, some chloromethyl groups still remain on the chloromethylated polysulfone, so as to ensure that the subsequently added tertiary amine compound B can react to introduce the R1 group.
[0027] It should also be noted that the reaction temperature for the quaternization reaction after adding the tertiary amine compound B is selected according to the specific tertiary amine compound actually selected, and the selected temperature should meet the requirements of accelerating the reaction while minimizing the volatilization of the tertiary amine. For example, when the tertiary amine compound B used is trimethylamine, the reaction temperature is 30-45°C and the reaction time is 8-24h. When the tertiary amine compound B is N,N-dimethylethylamine or N,N-dimethyl-n-propylamine or N,N-dimethyl-n-butylamine or N-methyl-n-pentylamine, the reaction temperature is 60-75°C and the reaction time is 8-24h.
[0028] It should also be noted that in order to ensure the product purity of the quaternary ammonium salt polysulfone obtained, the present invention also performs the following post-treatment on the reaction product obtained by the final quaternization reaction in step 2: the reaction product obtained by the quaternization reaction is distilled under reduced pressure and then dried to obtain the quaternary ammonium salt polysulfone.
[0029] Among them, the requirements for vacuum distillation are as follows:
[0030] If the amine that reacts with the chloromethyl polysulfone is a high-boiling-point amine, and the high-boiling-point amine is used in excess, after the reaction liquid is evaporated to dryness for the first time, a small amount of DMF needs to be added to the bottle, and after the solid is completely dissolved, the vacuum distillation is continued until the liquid is evaporated to dryness, and the steps of adding DMF to dissolve the solid and the vacuum distillation are repeated 2 to 3 times; then ethanol is added and the vacuum distillation is repeated 2 to 3 times, and the residual DMF and ethanol are removed by vacuum distillation together, and finally the reaction mixture is placed in a vacuum drying oven at 70 to 85°C for 12 to 24 hours to obtain the quaternary ammonium salt polysulfone with different side chain lengths.
[0031] If the amine reacting with the chloromethyl polysulfone is a low-boiling-point amine, after the reaction liquid is evaporated to dryness for the first time, water is added to dissolve the solid, and the vacuum distillation step is repeated 2 to 3 times, and the residual DMF and ethanol are removed by vacuum distillation together, and finally placed in a vacuum drying oven at 70 to 85° C. for 12 to 24 hours to obtain the quaternary ammonium polysulfone with different side chain lengths; if the prepared quaternary ammonium polysulfone is soluble in water, it is also possible not to place it in a vacuum drying oven, and the solid in the bottle is directly dissolved in water, and then frozen and dried to obtain a porous solid quaternary ammonium polysulfone.
[0032] The second object of the present invention is to provide a quaternary ammonium salt polysulfone prepared by the above preparation method.
[0033] The third object of the present invention is to provide an application of the quaternary ammonium salt polysulfone in the preparation of antibacterial materials.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] A long carbon chain quaternary ammonium salt functional group with high lipophilicity is introduced into the polysulfone structure, while a part of the short carbon chain quaternary ammonium salt functional group with good hydrophilicity is retained, so that the long carbon chain quaternary ammonium salt functional group is introduced into the polysulfone structure while maintaining its high water solubility, which is of great significance for regulating the hydrophilicity, antibacterial property and compatibility with other functional plastics of the polysulfone material. In addition, the preparation scheme provided by the invention is simple and has a high yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a macroscopic morphology photograph of the quaternary ammonium salt polysulfone prepared in Example 2.
[0037] Figure 2 This is the NMR image of the sample in Example 1.
[0038] Figure 3 This is the NMR image of the quaternary ammonium salt polysulfone prepared in Example 2.
[0039] Figure 4 This is the NMR image of the quaternary ammonium salt polysulfone prepared in Comparative Example 1.
[0040] Figure 5 This is the NMR image of the quaternary ammonium salt polysulfone prepared in Comparative Example 2.
[0041] Figure 6 This is the NMR image of the quaternary ammonium salt polysulfone prepared in Comparative Example 3.
[0042] Figure 7 This is the NMR image of the quaternary ammonium salt polysulfone prepared in Comparative Example 4. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention will be described clearly and completely below.
[0044] Example 1
[0045] This embodiment provides a quaternary ammonium salt polysulfone containing different side chain lengths, and it is prepared by the following steps:
[0046] Step 1, preparation of chloromethylated polysulfone:
[0047] 1) Place 20 g of polysulfone in 1000 mL of anhydrous chloroform, stir and heat to 50° C. at a stirring rate of 330 r / min, and then continue stirring at 50° C. for 2 h, at which time the polysulfone is completely dissolved to obtain a polysulfone solution.
[0048] 2) Dissolve 2 mL of anhydrous tin tetrachloride evenly in 20 mL of chloroform to obtain a tin tetrachloride solution.
[0049] 3) 18.0 g of paraformaldehyde and 100 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.5, the reaction was stopped.
[0050] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 1500 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0051] Step 2, compounding with tertiary amine compounds:
[0052] 1) Weigh 1.5 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF, and stir at a stirring rate of 330 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0053] 2) Under the protection of inert gas, 270 μL of N,N-dimethyl-n-octylamine was added to the chloromethylated polysulfone solution obtained above, and then the temperature was raised to 97° C. and the reaction was continued for 24 h to obtain an intermediate product.
[0054] 3) After the intermediate product is cooled to 40° C., 3 mL of a 30% trimethylamine aqueous solution is added, and then the reaction is continued at 40° C. for 12 h to obtain a reaction product.
[0055] 4) The reaction product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added, heated and stirred at 50° C. until a solution was obtained, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol was added and the distillation under reduced pressure was repeated 3 times to purify the reaction product. Finally, deionized water was added to dissolve, and the quaternary ammonium salt polysulfone product was obtained by freezing and drying, with a yield of 99.5%.
[0056] Example 2
[0057] This embodiment provides a quaternary ammonium salt polysulfone containing different side chain lengths, and it is prepared by the following steps:
[0058] Step 1, preparation of chloromethylated polysulfone:
[0059] 1) Place 10 g of polysulfone in 500 mL of anhydrous chloroform, heat to 50° C. with stirring at a stirring rate of 350 r / min, and then continue stirring at 50° C. for 60 min, at which time the polysulfone is completely dissolved to obtain a polysulfone solution.
[0060] 2) Dissolve 10 mL of anhydrous tin tetrachloride evenly in 10 mL of chloroform to obtain a tin tetrachloride solution.
[0061] 3) 9.0 g of paraformaldehyde and 50 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.6, the reaction was stopped.
[0062] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 600 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0063] Step 2, compounding with tertiary amine compounds:
[0064] 1) Weigh 2.15 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF. Stir at a stirring rate of 350 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0065] 2) Under the protection of inert gas, 650 μL of N,N-dimethyl-n-octylamine was added to the chloromethylated polysulfone solution obtained above, and then the temperature was raised to 97° C. and the reaction was continued for 24 h to obtain an intermediate product.
[0066] 3) After the intermediate product is cooled to 40° C., 3 mL of a 30% trimethylamine aqueous solution is added, and then the reaction is continued at 40° C. for 12 h to obtain a reaction product.
[0067] 4) The reaction product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added, heated and stirred at 50° C. until a solution was obtained, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol was added and the distillation under reduced pressure was repeated 3 times to purify the reaction product. Finally, deionized water was added to dissolve, and the quaternary ammonium salt polysulfone product was obtained by freezing and drying, with a yield of 99.6%.
[0068] Example 3
[0069] This embodiment provides a quaternary ammonium salt polysulfone containing different side chain lengths, and it is prepared by the following steps:
[0070] Step 1, preparation of chloromethylated polysulfone:
[0071] 1) Place 20 g of polysulfone in 1000 mL of anhydrous chloroform, stir and heat to 50° C. at a stirring rate of 340 r / min, and then continue stirring at 50° C. for 2 h, at which time the polysulfone is completely dissolved to obtain a polysulfone solution.
[0072] 2) 1.6 mL of anhydrous tin tetrachloride was uniformly dissolved in 15 mL of chloroform to obtain a tin tetrachloride solution.
[0073] 3) 18.0 g of paraformaldehyde and 100 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.5, the reaction was stopped.
[0074] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 1600 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0075] Step 2, compounding with tertiary amine compounds:
[0076] 1) Weigh 2.06 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF. Stir at a stirring rate of 340 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0077] 2) Under the protection of inert gas, 280 μL of N,N-dimethyl-n-octylamine was added to the chloromethylated polysulfone solution obtained above, and then the temperature was raised to 97° C. and reacted for 12 h to obtain an intermediate product.
[0078] 3) After the intermediate product was cooled to 60° C., 1.5 mL of N,N-dimethyl-n-butylamine was added, and then the reaction was continued at 60° C. for 12 h to obtain a reaction product.
[0079] 4) The reaction product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added, heated and stirred at 50° C. until a solution was obtained, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol was added and the distillation under reduced pressure was repeated 3 times to purify the reaction product. Finally, deionized water was added to dissolve, and the quaternary ammonium salt polysulfone product was obtained by freezing and drying, with a yield of 99.4%.
[0080] Comparative Example 1
[0081] This comparative example provides a quaternary ammonium salt polysulfone containing only one side chain length, and it is prepared by the following steps:
[0082] Step 1, preparation of chloromethylated polysulfone:
[0083] 1) 20 g of polysulfone was placed in 1000 mL of anhydrous chloroform, heated to 50° C. with stirring at a stirring rate of 340 r / min, and then continued to stir at 50° C. for 60 min, at which time the polysulfone was completely dissolved to obtain a polysulfone solution.
[0084] 2) 1.8 mL of anhydrous tin tetrachloride was uniformly dissolved in 20 mL of chloroform to obtain a tin tetrachloride solution.
[0085] 3) 18.0 g of paraformaldehyde and 100 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.5, the reaction was stopped.
[0086] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 1500 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0087] Step 2, compounding with tertiary amine compounds:
[0088] 1) Weigh 2.12 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF. Stir at a stirring rate of 340 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0089] 2) Under the protection of inert gas, 3 mL of a 30% trimethylamine aqueous solution was added to the chloromethylated polysulfone solution obtained above, and then the reaction was continued at 40° C. for 12 h to obtain a reaction product.
[0090] 3) The reaction product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added to the heated and stirred solution in the single-mouth bottle, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol and distillation under reduced pressure were continued for 3 times. Finally, a certain amount of water was added to the single-mouth bottle to dissolve, freeze and dry to obtain quaternary ammonium salt polysulfone, and the yield was 99.4%.
[0091] Comparative Example 2
[0092] This comparative example provides a quaternary ammonium salt polysulfone having only different side chain lengths, and is prepared by the following steps:
[0093] Step 1, preparation of chloromethylated polysulfone:
[0094] 1) Place 20 g of polysulfone in 1000 mL of anhydrous chloroform, heat to 50° C. with stirring at a stirring rate of 350 r / min, and then continue stirring at 50° C. for 2 h, at which time the polysulfone is completely dissolved to obtain a polysulfone solution.
[0095] 2) 1.8 mL of anhydrous tin tetrachloride was uniformly dissolved in 20 mL of chloroform to obtain a tin tetrachloride solution.
[0096] 3) 18.0 g of paraformaldehyde and 100 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.5, the reaction was stopped.
[0097] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 1500 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0098] Step 2, compounding with tertiary amine compounds:
[0099] 1) Weigh 2.05 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF. Stir at a stirring rate of 350 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0100] 2) Under the protection of inert gas, 2.0 mL of N,N-dimethyl-n-butylamine was added to the chloromethylated polysulfone solution obtained above, and then the temperature was raised to 97° C. and the reaction was continued for 24 h to obtain an intermediate product.
[0101] 3) The intermediate product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added to the heated and stirred solution in the single-mouth bottle, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol and distillation under reduced pressure were continued for 3 times. Finally, a certain amount of water was added to the single-mouth bottle to dissolve, and the quaternary ammonium salt polysulfone was obtained by freezing and drying, with a yield of 99.2%.
[0102] Comparative Example 3
[0103] This comparative example provides a quaternary ammonium salt polysulfone containing only one side chain length, and it is prepared by the following steps:
[0104] Step 1, preparation of chloromethylated polysulfone:
[0105] 1) Place 20 g of polysulfone in 1000 mL of anhydrous chloroform, stir and heat to 50° C. at a stirring rate of 330 r / min, and then continue stirring at 50° C. for 2 h, at which time the polysulfone is completely dissolved to obtain a polysulfone solution.
[0106] 2) 1.9 mL of anhydrous tin tetrachloride was uniformly dissolved in 20 mL of chloroform to obtain a tin tetrachloride solution.
[0107] 3) 18.0 g of paraformaldehyde and 100 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.5, the reaction was stopped.
[0108] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 1500 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0109] Step 2, compounding with tertiary amine compounds:
[0110] 1) Weigh 2.05 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF. Stir at a stirring rate of 330 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0111] 2) Under the protection of inert gas, 2.0 μL of N,N-dimethyl-n-hexylamine was added to the chloromethylated polysulfone solution obtained above, and then the temperature was raised to 97° C. and the reaction was continued for 24 h to obtain an intermediate product.
[0112] 3) The intermediate product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added to the heated and stirred solution in the single-mouth bottle, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol and distillation under reduced pressure were continued for 3 times. Finally, a certain amount of water was added to the single-mouth bottle to dissolve, and the quaternary ammonium salt polysulfone was obtained by freezing and drying, with a yield of 99.3%.
[0113] Comparative Example 4
[0114] This comparative example provides a quaternary ammonium salt polysulfone containing only one side chain length, and it is prepared by the following steps:
[0115] Step 1, preparation of chloromethylated polysulfone:
[0116] 1) Place 20 g of polysulfone in 1000 mL of anhydrous chloroform, stir and heat to 50° C. at a stirring rate of 340 r / min, and then continue stirring at 50° C. for 2 h, at which time the polysulfone is completely dissolved to obtain a polysulfone solution.
[0117] 2) 1.8 mL of anhydrous tin tetrachloride was uniformly dissolved in 20 mL of chloroform to obtain a tin tetrachloride solution.
[0118] 3) 18.0 g of paraformaldehyde and 100 mL of trimethylsilyl chloride were added to the polysulfone solution obtained above in sequence, and then, under nitrogen protection, the solution was slowly added dropwise to the tin tetrachloride solution obtained above. During the reaction, nuclear magnetic resonance detection was used for tracking. When the degree of chloromethylation substitution was 1.5, the reaction was stopped.
[0119] 4) After the reaction solution obtained in step 3) is cooled to room temperature, it is poured into 1500 mL of ethanol for precipitation, filtered, the precipitate is collected, and washed with anhydrous ethanol three times, and then placed in a vacuum drying oven at 50° C. and dried for 18 h to obtain chloromethylated polysulfone.
[0120] Step 2, compounding with tertiary amine compounds:
[0121] 1) Weigh 2.05 g of the chloromethylated polysulfone prepared in step 1 above and dissolve it in 50 mL of DMF. Stir at a stirring rate of 340 r / min for 20 min to obtain a chloromethylated polysulfone solution.
[0122] 2) Under the protection of inert gas, 2.0 mL of N,N-dimethyl-n-octylamine was added to the chloromethylated polysulfone solution obtained above, and then the temperature was raised to 97° C. and the reaction was continued for 24 h to obtain an intermediate product.
[0123] 3) The intermediate product was distilled under reduced pressure, evaporated to dryness, 50 mL of anhydrous ethanol was added to the heated and stirred solution in the single-mouth bottle, and the solution was distilled under reduced pressure to obtain a solid, and anhydrous ethanol and distillation under reduced pressure were continued for 3 times. Finally, a certain amount of water was added to the single-mouth bottle to dissolve, and the quaternary ammonium salt polysulfone was obtained by freezing and drying, with a yield of 99.6%.
[0124] Experimental Section
[0125] (I) Solubility test
[0126] The present invention takes the quaternary ammonium salt polysulfone prepared in Examples 1-3 and Comparative Examples 1-3 as examples, and uses water and anhydrous ethanol as solvents to test their solubility, and the test results are shown in Table 1.
[0127] It can be seen from the test results in Table 1 that the quaternary ammonium polysulfones obtained by introducing different R2 groups and R1 groups have different solubilities in water and anhydrous ethanol, which indicates that the present invention can adjust the solubility of the quaternary ammonium polysulfone in water and ethanol by regulating the molar ratio of the long side chain and the short side chain in the quaternary ammonium polysulfone.
[0128] Table 1 Solubility test results
[0129] water Anhydrous ethanol Example 1 Dissolve Emulsion Example 2 Dissolve Dissolve Example 3 Insoluble Dissolve Comparative Example 1 Dissolve Insoluble Comparative Example 2 Dissolve Insoluble Comparative Example 3 Dissolve Insoluble Comparative Example 4 Insoluble Dissolve
[0130] (II) Antibacterial performance test
[0131] The present invention takes the quaternary ammonium salt polysulfone prepared in Example 1 and Example 2 as examples, and tests the antibacterial properties thereof.
[0132] And the test method is as follows:
[0133] The quaternary ammonium salt polysulfone prepared in Example 1 and Example 2 were quantitatively weighed, sterilized by radiation, and dissolved in water to obtain a quaternary ammonium salt antibacterial solution. Escherichia coli ATCC25922 and Staphylococcus aureus ATCC25923 were prepared into bacterial suspensions with a concentration of 1.0×10 6 ~9.0×10 6 cfu / mL, 2.0 mL of sterilized tryptic soy broth (TSB), 400 μL of sterile water and 100 μL of bacterial suspension were added to test tube A (positive control group), 500 μL of sterile water and 2.0 mL of sterilized tryptic soy broth (TSB) were added to test tube B (negative control group), 2.0 mL of sterilized tryptic soy broth (TSB), 100 μL of bacterial suspension and 400 μL of quaternary ammonium polysulfone aqueous solution with a mass concentration of 1 wt% were added to test tube C (sample group), that is, The solubility of quaternary ammonium salt polysulfone is 1.6 mg / L. After being fully mixed, it is placed in an incubator at 37°C for 24 hours, and then appropriately diluted. Then, 2 to 3 dilutions are taken, 1 mL is respectively taken, and placed on 3 plates. Pour it with tryptic soy agar medium (TSA) cooled to 40 to 45°C, and the plates are rotated to make it fully uniform. After the agar solidifies, the plates are turned over and cultured at (35±2)°C for 48 hours. The live bacterial colonies are counted according to formula I, and good antibacterial effects are achieved against Escherichia coli ATCC25922 and Staphylococcus aureus ATCC25923.
[0134] The calculation formula of the antibacterial rate is shown in Formula I:
[0135]
[0136] Where:
[0137] X is the antibacterial rate, %;
[0138] A0 is the average colony count of the tested samples before shaking;
[0139] A1 is the average colony count of the test sample after shaking.
[0140] The above tests show that the antibacterial rates of the quaternary ammonium salt polysulfone prepared in Example 1 against Escherichia coli ATCC25922 and Staphylococcus aureus ATCC25923 are 99.9% and 95.3%, respectively.
[0141] The antibacterial rates of the quaternary ammonium salt polysulfone prepared in Example 2 against Escherichia coli ATCC25922 and Staphylococcus aureus ATCC25923 were 82.9% and 98.4%, respectively.
[0142] By comparing the test results of Example 2 with those of Example 1, it can be seen that a larger molar ratio of long carbon chain (N, N-dimethyl-n-octylamine) is introduced into the quaternary ammonium salt polysulfone of Example 2, so that it can be dissolved in both water and ethanol while maintaining a high antibacterial rate, and the antibacterial rate for different bacteria can be adjusted, thereby ultimately achieving the regulation of the comprehensive performance of the quaternary ammonium salt polysulfone.
[0143] (III) Morphology test
[0144] The present invention takes the quaternary ammonium salt polysulfone prepared in Example 2 as an example, and tests its macroscopic morphology, and the test results are as follows Figure 1 shown.
[0145] Figure 1 This is a macroscopic morphology photograph of the quaternary ammonium salt polysulfone prepared in Example 2. It can be seen that the quaternary ammonium salt polysulfone obtained in the present invention is a white solid.
[0146] (IV) MRI test
[0147] The present invention takes the quaternary ammonium salt polysulfone prepared in Examples 1-2 and Comparative Examples 1-4 as examples, and performs nuclear magnetic resonance verification on them, and the test results are as follows: Figure 2-7 shown.
[0148] Figure 2 and Figure 3 The NMR images of the quaternary ammonium salt polysulfone prepared in Example 1 and Example 2 are respectively different. Due to the different amounts of N,N-dimethyl-n-octylamine added for the first time, it can be seen from the integrated areas near the chemical shifts of 0.85 and 1.21 that they are significantly different, which are 0.94, 6.00 and 2.40, 13.34, respectively.
[0149] Figure 4 , Figure 5 , Figure 6 and Figure 7 The NMR images of the quaternary ammonium salt polysulfones prepared in Comparative Examples 1, 2, 3 and 4 respectively show that the chemical shift of the hydrogen on the methyl group linked to N is around 3.0-3.1. There are three methyl groups linked to N in the quaternary ammonium salt of Comparative Example 1, so the integral area (13.05) is relatively large, while there are only two methyl groups linked to N in the quaternary ammonium salts of Comparative Examples 2, 3 and 4, and the integral area (8.0-9.0) is relatively small when the degree of substitution of the chloromethyl group is substantially the same; with the introduction of a longer side chain on N, the chemical shift (1.69-1.70) of the hydrogen on the methyl group in the polysulfone main chain overlaps with the hydrogen on the methylene group in the longer side chain linked to N.
[0150] Based on the above, Figure 2-Figure 7 The NMR characterization results further prove that the present invention successfully introduces a long carbon chain quaternary ammonium salt functional group with high lipophilicity and a short carbon chain quaternary ammonium salt functional group with good hydrophilicity into the polysulfone structure to obtain a quaternary ammonium salt polysulfone with two different side chain lengths.
[0151] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing quaternary ammonium salt polysulfones containing different side chain lengths, characterized in that: The following steps are involved: Carrying out chloromethylation treatment on polysulfone to obtain chloromethylated polysulfone; The chloromethylated polysulfone is dissolved in a solvent, and under the protection of an inert gas, a tertiary amine compound A containing a carbon straight-chain alkyl group with a carbon number of ≥6 is added and mixed, and then a quaternization reaction is performed to introduce an R2 group on the chloromethylated polysulfone to obtain an intermediate product; a tertiary amine compound B containing a carbon straight-chain alkyl group with a carbon number of 1 to 5 is added to the intermediate product, and then a quaternization reaction is performed to introduce an R1 group on the intermediate product to obtain a quaternary ammonium salt polysulfone having both an R2 group and an R1 group as shown in formula I; Wherein, the R2 group is a carbon straight-chain alkyl group with a carbon number of ≥6; the R1 group is a carbon straight-chain alkyl group with a carbon number of 1 to 5.
2. The preparation method according to claim 1, characterized in that The R2 group is a straight-chain alkyl group having 6 to 8 carbon atoms; the R1 group is a straight-chain alkyl group having 1 to 4 carbon atoms.
3. The preparation method according to claim 1, characterized in that: The tertiary amine compound A is any one of N,N-dimethyl-n-hexylamine, N,N-dimethyl-n-heptylamine, N,N-dimethyl-n-octylamine and N,N-dimethyl tertiary amine having a straight-chain alkyl group with more than 8 carbon atoms.
4. The preparation method according to claim 1, characterized in that: The tertiary amine compound B is any one of trimethylamine, N,N-dimethylethylamine, N,N-dimethyl-n-propylamine, N,N-dimethyl-n-butylamine and N-methyl-n-pentylamine.
5. The preparation method according to claim 1, characterized in that: The molar ratio of the tertiary amine compound A to the tertiary amine compound B is 1:2-8; The molar ratio of the total molar amount of the tertiary amine compound A and the tertiary amine compound B to the chloromethylated polysulfone is 3 to 4:
1.
6. The preparation method according to claim 1, characterized in that: The reaction temperature for the quaternization reaction after adding the tertiary amine compound A is 30 to 100° C., and the reaction time is 8 to 24 hours.
7. The preparation method according to claim 1, characterized in that: The reaction temperature for the quaternization reaction after adding the tertiary amine compound B is 30 to 100° C., and the reaction time is 8 to 24 hours.
8. The preparation method according to claim 1, characterized in that: The solvent is any one of DMF, DMSO and NMP; The mass ratio of the tertiary amine compound A to the solvent is 1:20-30.
9. A quaternary ammonium salt polysulfone prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the quaternary ammonium salt polysulfone according to claim 9 in the preparation of antibacterial materials.