Copper-free ceramic friction material for brake pads and preparation method thereof
By modifying phenolic resin and basalt fiber, combined with silicon nitride and other materials, copper-free ceramic friction materials are prepared, which solves the problems of copper dust pollution and insufficient interface bonding strength, and improves the friction performance and heat resistance of the brake pads. Reduced noise.
Patent Information
- Application Number
- CN202410373360.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-29
AI Technical Summary
The copper contained in the existing brake pad friction materials leads to copper dust pollution, and the interface bonding strength and compatibility between the binder and the fiber substrate are insufficient, affecting the friction coefficient, wear resistance, thermal decay resistance and mechanical strength.
By modifying phenolic resin and basalt fiber to improve their compatibility and bonding strength, the modified phenolic resin and modified basalt fiber are used to synergize, combined with silicon nitride, sepiolite powder and other materials to prepare copper-free ceramic friction Material.
The mechanical strength, thermal decay resistance, wear resistance and friction coefficient of the friction material are significantly improved, friction noise is reduced, and copper dust pollution is avoided.
Smart Images

Figure BDA0004766278300000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automobile friction brake materials, and in particular relates to a copper-free ceramic friction material for brake pads and a preparation method thereof. Background Art
[0002] Brake pads are also called brake pads or brake leathers. Brake pads are the most critical safety parts in the vehicle's braking system. The quality of all braking effects is determined by brake pads. Brake pads are generally composed of steel plates, adhesive insulation layers and friction blocks. Among them, the friction block is composed of friction material and adhesive. When braking, it is squeezed on the brake disc or brake drum to generate friction, thereby achieving the purpose of vehicle deceleration and braking. Friction material is a composite material with friction as its main function and structural performance requirements. The braking performance is closely related to the degree of wear of the friction material in the friction block. The quality of the friction material directly affects the reliability and safety of the automobile brake pad. Therefore, the friction material needs to have a stable friction coefficient, good wear resistance and mechanical strength, and low noise.
[0003] The Chinese patent with publication number CN115322587A discloses a friction material for disc brakes, a preparation method and application thereof, wherein the friction material for disc brakes comprises a fiber substrate, an adhesive and a friction performance modifier, and the adhesive comprises an organic sodium salt; the organic sodium salt is selected as an adhesive in combination with the fiber substrate and the friction performance modifier, which can effectively improve the dispersibility of the friction material, and at the same time, by changing the surface energy of the friction material, the recovery of the disc brake pad prepared by the friction material after wading is improved, making it more suitable for use in off-road vehicles. The Chinese patent with publication number CN113217569B discloses a brake pad friction material, a brake pad friction block, a preparation method thereof and a brake pad. In the brake pad friction material of the invention, phenolic resin is used as the main binder, and nitrile rubber powder is used to assist bonding. The mass fraction of phenolic resin in the brake pad friction material is 4.0% to 7.0%, which is a relatively low content. Zirconium silicate, antimony sulfide and electrolytic copper powder are added to the raw materials. Zirconium silicate, antimony sulfide and electrolytic copper powder are heated by friction in the friction interface layer, so that oxidative decomposition occurs when phenolic resin and the like undergo thermal decomposition, thereby playing a bonding role in the high-temperature stage. In addition, zirconium silicate, antimony sulfide and electrolytic copper powder can work synergistically to ensure that the brake pad friction material can maintain a stable friction coefficient in both the low-temperature stage and the high-temperature stage, and the cost is low. However, the brake pad friction materials in the above-mentioned prior art all contain copper, and the copper-containing friction materials will discharge copper in the form of wear powder when the vehicle brakes, resulting in a large amount of copper dust being generated as the friction materials wear. These copper dusts will eventually flow into rivers, lakes, oceans and other waters and deposit in the water, thereby causing heavy metal copper pollution in the water body; and the interface bonding strength and compatibility between the binder and the fiber substrate in the brake pad friction materials in the above-mentioned prior art need to be further improved, which affects the friction coefficient, wear resistance, thermal decay resistance, mechanical strength and other properties of the brake pad friction materials. Therefore, it is a technical problem that needs to be solved urgently to study a kind of excellent interface strength and compatibility between the binder and the fiber substrate, so that the copper-free friction material for the brake pad has a stable friction coefficient, good wear resistance and mechanical strength, thermal decay resistance and low noise. Summary of the invention
[0004] In order to solve the deficiencies in the prior art, the purpose of the present invention is to provide a copper-free ceramic friction material for brake pads and a preparation method thereof. By modifying phenolic resin and basalt fiber, the compatibility and bonding strength between basalt fiber and phenolic resin matrix are improved, and the modified phenolic resin and modified basalt fiber are synergistically enhanced, which significantly improves the mechanical strength, thermal decay resistance, wear resistance and friction coefficient of the friction material.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A copper-free ceramic friction material for a brake pad. The raw materials of the friction material include the following components in parts by weight: 15-25 parts of modified phenolic resin, 12-18 parts of short pre-oxidized filaments, 3-8 parts of aramid pulp, 6-12 parts of basalt fiber, 4-8 parts of silicon nitride, 2-4 parts of sepiolite powder, 6-10 parts of zirconium silicate, 3-5 parts of barium sulfate, 4-6 parts of zircon powder, 1-3 parts of coke powder, 1-3 parts of graphite powder, 2-5 parts of potassium titanate, 2-4 parts of tire powder and 3-6 parts of zinc powder.
[0007] Furthermore, the modified phenolic resin is prepared by the following steps:
[0008] 1) dispersing molybdenum disulfide powder in water, adding 3-mercapto-1,2-propylene glycol, ultrasonically dispersing for 2-6 hours, then mechanically stirring for 24-30 hours, filtering, and obtaining hydroxylated molybdenum disulfide;
[0009] 2) adding hexadecyltrimethoxysilane, polyvinylpyrrolidone, sodium dodecylbenzenesulfonate and water into a reaction vessel, stirring at a speed of 600-800 r / min for 40-60 min, then adding an appropriate amount of triethylamine, continuing to stir and react for 12-15 h, and after the reaction is completed, centrifuging, filtering and washing the reaction product to obtain polysiloxane microspheres;
[0010] 3) The phenol and formaldehyde dispersions are mixed uniformly, and the pH is adjusted to 7.5-8 with ammonia water under stirring conditions, and the temperature is raised to 70-80° C. and stirred for reaction for 1.5-2 hours, and then the temperature is raised to 90-105° C. and stirred for reaction for 2-3 hours, and then the hydroxylated molybdenum disulfide obtained in step 1), 3-aminopropyltrimethoxysilane and the polysiloxane microspheres obtained in step 2) are added thereto in sequence, and the mixture is stirred for another 6-10 hours. After the reaction is completed, the reaction product is cooled to room temperature and filtered, and the filter cake is washed with anhydrous ethanol for 3-5 times, and placed in a vacuum drying oven at 60-80° C. and dried for 3-5 hours to obtain a modified phenolic resin.
[0011] Furthermore, in the step 1), the mass ratio of molybdenum disulfide powder, water and 3-mercapto-1,2-propylene glycol is (0.5-0.8):(50-400):(1.5-20).
[0012] Furthermore, in the step 2), the mass ratio of hexadecyltrimethoxysilane, polyvinylpyrrolidone, sodium dodecylbenzenesulfonate and water is (150-220):(0.8-2.5):(0.4-1):(600-900).
[0013] Furthermore, in the step 3), the molar ratio of phenol, formaldehyde, 3-aminopropyltrimethoxysilane and hydroxylated molybdenum disulfide is (0.8-1.2):(1.2-1.3):(0.1-0.15):(0.02-0.03).
[0014] Specifically, due to its shortcomings such as high brittleness and poor high-temperature heat resistance, phenolic resin, when used as a binder for brake pad friction materials, will affect the heat resistance, friction performance and mechanical properties of the friction materials. Therefore, the phenolic resin needs to be modified. The present application modifies phenolic resin by using coupling agent 3-aminopropyltrimethoxysilane, hydroxylated molybdenum disulfide grafting and polysiloxane microspheres to obtain phenolic resin co-modified with molybdenum disulfide and polysiloxane microspheres; firstly, molybdenum disulfide is hydroxylated, and hydroxylated molybdenum disulfide is conducive to subsequent grafting reaction with phenolic resin, and then 3-aminopropyltrimethoxysilane is used to graft hydroxylated molybdenum disulfide onto phenolic resin, so that oxygen-molybdenum bonds are grafted into phenolic resin molecules, thereby improving the high-temperature heat resistance and thermal stability of phenolic resin; at the same time, polysiloxane microspheres have many pores, and after adding polysiloxane microspheres to phenolic resin, many microporous structures with excellent mechanical properties can be introduced into the phenolic resin, so that the phenolic resin has excellent flexibility. Therefore, after co-modification with molybdenum disulfide and polysiloxane microspheres, the high-temperature heat resistance and toughness of phenolic resin are improved, thereby improving the heat resistance and mechanical strength of friction materials, and stabilizing the friction coefficient of friction materials and reducing the wear rate.
[0015] Furthermore, the basalt fiber has a diameter of 3-8 μm and a length of 1-3.5 mm.
[0016] Furthermore, the basalt fiber is a modified basalt fiber, and the preparation method of the modified basalt fiber specifically comprises the following steps:
[0017] (1) dissolving γ-aminopropyltriethoxysilane in a mixture of water and anhydrous ethanol, stirring for 10-20 minutes to mix them evenly, to obtain a γ-aminopropyltriethoxysilane hydrolyzate; the volume ratio of water to anhydrous ethanol in the mixture of water and anhydrous ethanol is (2:8)-(3:7);
[0018] (2) adding basalt fiber to the γ-aminopropyltriethoxysilane hydrolyzate obtained in step (1), stirring for 40-60 minutes to obtain a mixed solution 1, then adding a rare earth cerium chloride solution to the mixed solution 1, continuing to stir for 30-40 minutes, filtering, first naturally airing at room temperature for 20-30 hours, and then drying in a vacuum drying oven at 100-120° C. for 1-2 hours to obtain modified basalt fiber; wherein the mass ratio of the basalt fiber, the γ-aminopropyltriethoxysilane hydrolyzate and the rare earth cerium chloride is 1:(3.5-6.5):(2-3); the mass percentage of the rare earth cerium chloride in the rare earth cerium chloride solution is 12-15%; and the mass percentage of the γ-aminopropyltriethoxysilane in the γ-aminopropyltriethoxysilane hydrolyzate is 0.9-1.5%.
[0019] Specifically, the present application first modifies the surface of basalt fiber by using the coupling agent γ-aminopropyl triethoxysilane hydrolyzate, and then obtains basalt fiber co-modified by coupling agent and rare earth cerium chloride through the coupling effect between the coupling agent and the rare earth element. After hydrolysis of γ-aminopropyl triethoxysilane, silanol bonds are formed, and the silanol bonds are bonded with the hydroxyl groups on the surface of the basalt fiber to form Si-O-Si bonds, so that the coupling agent γ-aminopropyl triethoxysilane is grafted onto the surface of the basalt fiber. The surface of the basalt fiber grafted with γ-aminopropyl triethoxysilane contains a large number of active end-capping groups such as amino groups and hydroxyl groups, which can undergo grafting or block copolymerization reactions with groups such as hydroxymethyl in the structure of the phenolic resin, thereby improving the interface compatibility and bonding strength between the basalt fiber and the phenolic resin; at the same time, the rare earth Ce 3+ It can form a coordination bond with the oxygen on the hydroxyl group in the phenolic resin molecule to obtain a stable rare earth complex, so that the basalt fiber and the phenolic resin are chemically bonded together through the rare earth element Ce, thereby improving the interface bonding strength between the basalt fiber and the phenolic resin, and further enhancing the mechanical strength of the friction material; and the rare earth element Ce can penetrate into the phenolic resin matrix, and can also react with the sulfur element in the molybdenum disulfide in the modified phenolic resin to form a stable chemical friction film, further improving the interface bonding force between the basalt fiber and the phenolic resin, thereby improving the wear resistance and mechanical properties of the friction material; and the heat resistance of the basalt fiber modified by the rare earth is improved, so that the carbonization degree of the basalt fiber in the high-temperature friction process is greatly reduced, so that the basalt fiber can still maintain the reinforcing effect on the friction material at high temperature, further improving the high temperature resistance of the friction material, so the modified basalt fiber can effectively improve the friction coefficient of the friction material and the stability of the friction coefficient, thereby improving the heat decay resistance of the friction material.
[0020] Furthermore, the method for preparing the copper-free ceramic friction material for the brake pad comprises the following steps:
[0021] Step S1, weighing each raw material according to the above weight parts;
[0022] Step S2, placing the raw materials weighed in step S1 into a mixer according to corresponding weight portions and mixing them evenly to obtain a mixed raw material, wherein the main shaft speed of the mixer is 160-220 r / min, the reamer speed is 1900-2700 r / min, and the mixing time is 160-240 s;
[0023] Step S3, pressing and heat treating the mixed raw materials obtained in step S2 in sequence to obtain the copper-free ceramic friction material for the brake pad.
[0024] Furthermore, the specific steps of pressing in step S3 are as follows: pressing the mixed raw materials through a hot press, the pressing temperature is 120-130°C, the feeding amount is 195-200g each time; the pressing pressure is 40-50bar; the air is released after pressing for 2-4s, the air release time is 2-5s, the air release is repeated 3 times, and the final pressure holding time is 160-180s, and the vacuum degree is 3-5bar.
[0025] Furthermore, the specific steps of the heat treatment in step S3 are as follows: first heat up to 140-150°C, keep warm for 50-60min, then heat up to 150-160°C, keep warm for 60-70min, then heat up to 170-180°C, keep warm for 60-70min, then heat up to 190-200°C, keep warm for 120-140min, finally heat up to 210-230°C, keep warm for 150-200min, and the heating rate is 8-10min / °C.
[0026] Compared with the prior art, the present invention has the following positive and beneficial effects:
[0027] (1) The present invention modifies phenolic resin by using coupling agent 3-aminopropyltrimethoxysilane, hydroxylated molybdenum disulfide grafting and polysiloxane microspheres to obtain phenolic resin co-modified with molybdenum disulfide and polysiloxane microspheres; firstly, molybdenum disulfide is hydroxylated, and then 3-aminopropyltrimethoxysilane is used to graft hydroxylated molybdenum disulfide onto the phenolic resin, so that oxygen-molybdenum bonds are grafted into the phenolic resin molecules, thereby improving the high-temperature heat resistance and thermal stability of the phenolic resin; at the same time, the polysiloxane microspheres have many pores, and after the polysiloxane microspheres are added to the phenolic resin, they can be introduced into the phenolic resin. The microporous structure with many excellent mechanical properties makes the phenolic resin have excellent flexibility, and the microporous structure can also effectively block the propagation of sound waves. Part of the friction sound energy will be reflected back by the micropores, so that the phenolic resin has a good noise reduction effect, thereby reducing the friction noise of the friction material; therefore, the high temperature heat resistance and toughness of the phenolic resin are improved after co-modification with molybdenum disulfide and polysiloxane microspheres, and the phenolic resin has a good noise reduction effect, thereby improving the mechanical strength of the friction material, stabilizing the friction coefficient of the friction material, reducing the wear rate, and reducing the friction noise of the friction material.
[0028] (2) The present invention first modifies the surface of basalt fiber by using the coupling agent γ-aminopropyl triethoxysilane hydrolyzate, and then obtains basalt fiber co-modified with the coupling agent and rare earth cerium chloride through the coupling effect between the coupling agent and the rare earth element; γ-aminopropyl triethoxysilane is hydrolyzed to form silanol bonds, and the silanol bonds are bonded with the hydroxyl groups on the surface of the basalt fiber to form Si-O-Si bonds, so that the coupling agent γ-aminopropyl triethoxysilane is grafted onto the surface of the basalt fiber. The surface of the basalt fiber grafted with γ-aminopropyl triethoxysilane contains a large number of active end-capping groups such as amino groups and hydroxyl groups, which can undergo grafting or block copolymerization reactions with groups such as hydroxymethyl in the structure of the phenolic resin, thereby improving the compatibility and bonding strength between the basalt fiber and the phenolic resin; at the same time, the rare earth Ce 3+ It can form a coordination bond with the oxygen on the hydroxyl group in the phenolic resin molecule to obtain a stable rare earth complex, so that the basalt fiber and the phenolic resin are chemically bonded together through the rare earth element Ce, thereby improving the interface bonding strength between the basalt fiber and the phenolic resin, and further enhancing the mechanical strength of the friction material; and the rare earth element Ce can penetrate into the phenolic resin matrix, and can also react with the sulfur element in the molybdenum disulfide in the modified phenolic resin to form a stable chemical friction film, thereby improving the interface bonding force between the basalt fiber and the phenolic resin, thereby improving the wear resistance and mechanical properties of the friction material; the heat resistance of the modified basalt fiber is improved, so that the carbonization degree of the basalt fiber in the high-temperature friction process is greatly reduced, so that the basalt fiber can still maintain the reinforcing effect on the friction material at high temperature, further improving the high temperature resistance of the friction material, so the basalt fiber modified by rare earth can effectively improve the friction coefficient of the friction material and the stability of the friction coefficient, thereby improving the heat decay resistance of the friction material. Therefore, the present invention improves the compatibility and bonding strength between the basalt fiber and the phenolic resin matrix by modifying the phenolic resin and basalt fiber. The modified phenolic resin and the modified basalt fiber synergize with each other, thereby significantly improving the mechanical strength, heat decay resistance, wear resistance and friction coefficient of the friction material.
[0029] (3) The present invention uses silicon nitride, sepiolite powder, zirconium silicate, barium sulfate, zircon powder, coke powder, graphite powder, potassium titanate, tire powder and zinc powder as friction modifiers and fillers of friction materials, and uses high, medium and low hardness friction modifiers and fillers in combination, thereby improving the wear resistance and friction coefficient stability of the friction material; and zinc powder is a low-melting point soft metal with good ductility and thermal conductivity, which can increase the actual friction contact area of the friction material. During the friction process, a friction film is also formed on the surface of the brake pad, which is beneficial to reducing the probability of friction noise, and can also stabilize the friction coefficient of the friction material and reduce the amount of wear. DETAILED DESCRIPTION
[0030] The technical solution of the present application will be described clearly and completely in conjunction with the following embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0031] In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. All reagents used without special instructions are conventional reagents used in the art, and all reagents or instruments used without specifying the manufacturer are conventional products that can be purchased commercially.
[0032] Example 1
[0033] The preparation method of the modified phenolic resin comprises the following steps:
[0034] 1) dispersing molybdenum disulfide powder in water, adding 3-mercapto-1,2-propylene glycol, ultrasonically dispersing for 2-6 hours, then mechanically stirring for 24-30 hours, filtering, and obtaining hydroxylated molybdenum disulfide; wherein the mass ratio of molybdenum disulfide powder, water, and 3-mercapto-1,2-propylene glycol is (0.5-0.8):(50-400):(1.5-20);
[0035] 2) adding hexadecyltrimethoxysilane, polyvinylpyrrolidone, sodium dodecylbenzenesulfonate and water into a reaction vessel, stirring at a speed of 600-800 r / min for 40-60 min, then adding an appropriate amount of triethylamine, continuing to stir and react for 12-15 h, and after the reaction is completed, centrifuging, filtering and washing the reaction product to obtain polysiloxane microspheres; wherein the mass ratio of hexadecyltrimethoxysilane, polyvinylpyrrolidone, sodium dodecylbenzenesulfonate and water is (150-220):(0.8-2.5):(0.4-1):(600-900);
[0036] 3) Mix the phenol and formaldehyde dispersions uniformly, adjust the pH to 7.5-8 with ammonia water under stirring, heat to 70-80°C and stir for reaction for 1.5-2h, heat to 90-105°C and continue stirring for reaction for 2-3h, then add the hydroxylated molybdenum disulfide obtained in step 1), 3-aminopropyltrimethoxysilane and polysiloxane microspheres obtained in step 2) in sequence, and react for another 6-10h under stirring. After the reaction is completed, cool the reaction product to room temperature and filter, wash the filter cake with anhydrous ethanol for 3-5 times, and place it in a vacuum drying oven at 60-80°C and dry it for 3-5h to obtain a modified phenolic resin. The molar ratio of phenol, formaldehyde, 3-aminopropyltrimethoxysilane to hydroxylated molybdenum disulfide is (0.8-1.2):(1.2-1.3):(0.1-0.15):(0.02-0.03).
[0037] Example 2
[0038] The basalt fiber used in the following examples and comparative examples of the present application is modified basalt fiber, and the preparation method of the modified basalt fiber specifically includes the following steps:
[0039] (1) dissolving γ-aminopropyltriethoxysilane in a mixture of water and anhydrous ethanol, stirring for 10-20 minutes to mix them evenly, to obtain a γ-aminopropyltriethoxysilane hydrolyzate; the volume ratio of water to anhydrous ethanol in the mixture of water and anhydrous ethanol is (2:8)-(3:7);
[0040] (2) adding basalt fiber to the γ-aminopropyltriethoxysilane hydrolyzate obtained in step (1), stirring for 40-60 minutes to obtain a mixed solution 1, then adding a rare earth cerium chloride solution to the mixed solution 1, continuing to stir for 30-40 minutes, filtering, first naturally airing at room temperature for 20-30 hours, and then drying in a vacuum drying oven at 100-120° C. for 1-2 hours to obtain modified basalt fiber. Wherein, the mass ratio of the basalt fiber, the γ-aminopropyltriethoxysilane hydrolyzate and the rare earth cerium chloride is 1:(3.5-6.5):(2-3); the mass percentage of the rare earth cerium chloride in the rare earth cerium chloride solution is 12-15%; the mass percentage of the γ-aminopropyltriethoxysilane in the γ-aminopropyltriethoxysilane hydrolyzate is 0.9-1.5%.
[0041] The modified phenolic resin and basalt fiber used in the following examples and comparative examples were prepared by the methods of Example 1 and Example 2, respectively.
[0042] The basalt fibers used in the following examples and comparative examples have a diameter of 3-8 μm and a length of 1-3.5 mm.
[0043] Example 3
[0044] A copper-free ceramic friction material for a brake pad. The raw materials of the friction material, measured in parts by weight, include the following components: 15 parts of modified phenolic resin, 12 parts of short pre-oxidized filaments, 3 parts of aramid pulp, 6 parts of basalt fiber, 4 parts of silicon nitride, 2 parts of sepiolite powder, 8 parts of zirconium silicate, 4 parts of barium sulfate, 4 parts of zircon powder, 1 part of coke powder, 2 parts of graphite powder, 2 parts of potassium titanate, 3 parts of tire powder and 3 parts of zinc powder.
[0045] A method for preparing a copper-free ceramic friction material for a brake pad comprises the following steps:
[0046] Step S1, weighing each raw material according to the above weight parts;
[0047] Step S2, placing the raw materials weighed in step S1 into a mixer according to corresponding weight portions and mixing them evenly to obtain a mixed raw material, wherein the main shaft speed of the mixer is 160 r / min, the reamer speed is 1900 r / min, and the mixing time is 240 s;
[0048] Step S3, the mixed raw materials obtained in step S2 are pressed and heat treated in sequence to obtain copper-free ceramic friction materials for brake pads; the specific steps of pressing are as follows: the mixed raw materials are pressed by a hot press, the pressing temperature is 120°C, and the feeding amount is 195g each time; the pressing pressure is 40bar; the air is released after pressing for 2s, the air release time is 2s, and the air release is repeated 3 times, and the final pressure holding time is 160s, and the vacuum degree is 3bar; the specific steps of heat treatment are as follows: first heat up to 140°C, keep warm for 60min, then heat up to 150°C, keep warm for 70min, then heat up to 170°C, keep warm for 70min, then heat up to 190°C, keep warm for 140min, and finally heat up to 210°C, keep warm for 200min, and the heating rate is 8min / °C.
[0049] Example 4
[0050] A copper-free ceramic friction material for a brake pad. The raw materials of the friction material, measured in parts by weight, include the following components: 20 parts of modified phenolic resin, 15 parts of short pre-oxidized filaments, 5 parts of aramid pulp, 10 parts of basalt fiber, 6 parts of silicon nitride, 3 parts of sepiolite powder, 6 parts of zirconium silicate, 3 parts of barium sulfate, 5 parts of zircon powder, 2 parts of coke powder, 3 parts of graphite powder, 3 parts of potassium titanate, 2 parts of tire powder and 5 parts of zinc powder.
[0051] A method for preparing a copper-free ceramic friction material for a brake pad comprises the following steps:
[0052] Step S1, weighing each raw material according to the above weight parts;
[0053] Step S2, placing the raw materials weighed in step S1 into a mixer according to the corresponding weight portions and mixing them evenly to obtain a mixed raw material, wherein the main shaft speed of the mixer is 200 r / min, the reamer speed is 2400 r / min, and the mixing time is 200 s;
[0054] Step S3, the mixed raw materials obtained in step S2 are pressed and heat treated in sequence to obtain copper-free ceramic friction materials for brake pads; the specific steps of pressing are as follows: the mixed raw materials are pressed by a hot press, the pressing temperature is 125°C, and the feeding amount is 198g each time; the pressing pressure is 45bar; the air is released after pressing for 3s, the air release time is 4s, and the air release is repeated 3 times, and the final pressure holding time is 170s, and the vacuum degree is 4bar; the specific steps of heat treatment are as follows: first heat up to 145°C, keep warm for 55min, then heat up to 155°C, keep warm for 65min, then heat up to 175°C, keep warm for 65min, then heat up to 195°C, keep warm for 130min, and finally heat up to 220°C, keep warm for 180min, and the heating rate is 9min / °C.
[0055] Example 5
[0056] A copper-free ceramic friction material for a brake pad. The raw materials of the friction material, measured in parts by weight, include the following components: 25 parts of modified phenolic resin, 18 parts of short pre-oxidized filaments, 8 parts of aramid pulp, 12 parts of basalt fiber, 8 parts of silicon nitride, 4 parts of sepiolite powder, 10 parts of zirconium silicate, 5 parts of barium sulfate, 6 parts of zircon powder, 3 parts of coke powder, 1 part of graphite powder, 5 parts of potassium titanate, 4 parts of tire powder and 6 parts of zinc powder.
[0057] A method for preparing a copper-free ceramic friction material for a brake pad comprises the following steps:
[0058] Step S1, weighing each raw material according to the above weight parts;
[0059] Step S2, placing the raw materials weighed in step S1 into a mixer according to the corresponding weight portions and mixing them evenly to obtain a mixed raw material, wherein the main shaft speed of the mixer is 220 r / min, the reamer speed is 2700 r / min, and the mixing time is 160 s;
[0060] Step S3, the mixed raw materials obtained in step S2 are pressed and heat treated in sequence to obtain copper-free ceramic friction materials for brake pads; the specific steps of pressing are as follows: the mixed raw materials are pressed by a hot press, the pressing temperature is 130°C, and the feeding amount is 200g each time; the pressing pressure is 50bar; the air is released after pressing for 4s, the air release time is 5s, and the air release is repeated 3 times, and the final pressure is maintained for 180s, and the vacuum degree is 5bar; the specific steps of heat treatment are as follows: first heat up to 150°C, keep warm for 50min, then heat up to 160°C, keep warm for 60min, then heat up to 180°C, keep warm for 70min, then heat up to 200°C, keep warm for 120min, and finally heat up to 230°C, keep warm for 150min, and the heating rate is 10min / °C.
[0061] Comparative Example 1
[0062] In this comparative example, the copper-free ceramic friction material for brake pads is exactly the same as that in Example 4 except that the modified phenolic resin is replaced by an equal amount of ordinary unmodified phenolic resin. Other raw material components and the preparation method of the copper-free ceramic friction material for brake pads are exactly the same as those in Example 4.
[0063] Comparative Example 2
[0064] In this comparative example, the copper-free ceramic friction material for brake pads is exactly the same as that in Example 4 except that the modified phenolic resin is replaced by an equal amount of phenolic resin modified only with molybdenum disulfide. Other raw material components and the preparation method of the copper-free ceramic friction material for brake pads are exactly the same as those in Example 4.
[0065] Comparative Example 3
[0066] In this comparative example, the copper-free ceramic friction material for brake pads is exactly the same as that in Example 4 except that the basalt fiber is replaced with an equal amount of ordinary unmodified basalt fiber. Other raw material components and the preparation method of the copper-free ceramic friction material for brake pads are exactly the same as those in Example 4.
[0067] Comparative Example 4
[0068] In this comparative example, the copper-free ceramic friction material for brake pads is exactly the same as that in Example 4 except that the basalt fiber is replaced with an equal amount of basalt fiber modified only with γ-aminopropyltriethoxysilane. Other raw material components and the preparation method of the copper-free ceramic friction material for brake pads are exactly the same as those in Example 4.
[0069] Test example
[0070] The copper-free ceramic friction materials for brake pads prepared in Examples 3-5 and Comparative Examples 1-4 were subjected to hardness, noise, normal temperature shear, normal temperature compression, normal temperature bending and friction tests, and the specific test results are shown in Table 1. Among them, the test standard for hardness test is GB / T3398.2-2008, and the hardness standard is Rockwell hardness HRL; the test standard for noise is tested according to SAEJ2521 test noise; the test standard for normal temperature shear test is GB / T22309; the test standard for normal temperature compression test is GB / T34559-2017; the test standard for normal temperature bending test is GB / T6569-2006; the friction performance is tested according to the method in SAE2522, and the friction performance includes average friction coefficient, first decay friction coefficient, second decay friction coefficient and weight wear.
[0071] Table 1 Performance test data of copper-free ceramic friction materials for brake pads prepared in Examples 3-5 and Comparative Examples 1-4
[0072]
[0073] It can be seen from the data in Table 1 that the hardness, noise, mechanical properties (shear strength, compression strength, bending strength), wear resistance, friction coefficient, thermal decay and other properties of the copper-free ceramic friction materials for brake pads prepared in Examples 3-5 of the present application are better than those in Comparative Examples 1-4. This is mainly because the present application improves the compatibility and bonding strength between the basalt fiber and the phenolic resin matrix by modifying the phenolic resin and basalt fiber, and the modified phenolic resin and the modified basalt fiber synergize with each other, thereby significantly improving the mechanical strength, thermal decay resistance, wear resistance and friction coefficient of the friction material. By comparing Comparative Examples 1-2 with Example 4, it can be found that the present application modifies the phenolic resin by using a coupling agent 3-aminopropyltrimethoxysilane, hydroxylated molybdenum disulfide grafting and polysiloxane microspheres to obtain a phenolic resin co-modified with molybdenum disulfide and polysiloxane microspheres; firstly, molybdenum disulfide is hydroxylated, and then 3-aminopropyltrimethoxysilane is used to graft the hydroxylated molybdenum disulfide onto the phenolic resin, so that oxygen-molybdenum bonds are grafted into the phenolic resin molecules, thereby improving the high temperature heat resistance and thermal stability of the phenolic resin; at the same time, the polysiloxane microspheres have many pores, and the polysiloxane microspheres can be added to the phenolic resin. Many microporous structures with excellent mechanical properties are introduced into the phenolic resin, which makes the phenolic resin have excellent flexibility. The microporous structure can also effectively block the propagation of sound waves. Part of the friction sound energy will be reflected back by the micropores, so that the phenolic resin has a good noise reduction effect, thereby reducing the friction noise of the friction material; therefore, the high temperature heat resistance and toughness of the phenolic resin are improved through co-modification with molybdenum disulfide and polysiloxane microspheres, and the phenolic resin has a good noise reduction effect, thereby improving the mechanical strength of the friction material, making the friction coefficient of the friction material stable, the wear rate low, and reducing the friction noise of the friction material.By comparing Comparative Examples 3-4 with Example 4, it is found that the present application first modifies the surface of the basalt fiber by using the coupling agent γ-aminopropyltriethoxysilane hydrolyzate, and then obtains the basalt fiber co-modified with the coupling agent and rare earth cerium chloride through the coupling effect between the coupling agent and the rare earth element; γ-aminopropyltriethoxysilane forms a silanol bond after hydrolysis, and the silanol bond bonds with the hydroxyl groups on the surface of the basalt fiber to form a Si-O-Si bond, so that the coupling agent γ-aminopropyltriethoxysilane is grafted onto the surface of the basalt fiber. The surface of the basalt fiber grafted with γ-aminopropyltriethoxysilane contains a large number of active end-capping groups such as amino groups and hydroxyl groups, which can undergo grafting or block copolymerization reactions with groups such as hydroxymethyl in the phenolic resin structure, thereby improving the compatibility and bonding strength between the basalt fiber and the phenolic resin; at the same time, the rare earth Ce3+ can form a coordination bond with the oxygen on the hydroxyl group in the phenolic resin molecule to obtain a stable rare earth coordination bond. The basalt fiber and the phenolic resin are chemically bonded together through the rare earth element Ce, thereby improving the interface bonding strength between the basalt fiber and the phenolic resin, and further enhancing the mechanical strength of the friction material; and the rare earth element Ce can penetrate into the phenolic resin matrix, and can also react with the sulfur element in the molybdenum disulfide in the modified phenolic resin to form a stable chemical friction film, thereby improving the interface bonding force between the basalt fiber and the phenolic resin, thereby improving the wear resistance and mechanical properties of the friction material; the heat resistance of the modified basalt fiber is improved, so that the carbonization degree of the basalt fiber in the high-temperature friction process is greatly reduced, so that the basalt fiber can still maintain the reinforcing effect on the friction material at high temperature, further improving the high temperature resistance of the friction material, so the modified basalt fiber can effectively improve the friction coefficient of the friction material and the stability of the friction coefficient, thereby improving the heat decay resistance of the friction material. Therefore, the present invention improves the compatibility and bonding strength between the basalt fiber and the phenolic resin matrix by modifying the phenolic resin and basalt fiber. The modified phenolic resin and the modified basalt fiber synergize with each other, thereby significantly improving the mechanical strength, heat decay resistance, wear resistance and friction coefficient of the friction material.
[0074] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0075] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A copper-free ceramic friction material for brake pads, characterized in that: The raw materials of the friction material include the following components in parts by weight: 15-25 parts of modified phenolic resin, 12-18 parts of short pre-oxidized fibers, 3-8 parts of aramid pulp, 6-12 parts of basalt fibers, 4-8 parts of silicon nitride, 2-4 parts of sepiolite powder, 6-10 parts of zirconium silicate, 3-5 parts of barium sulfate, 4-6 parts of zircon powder, 1-3 parts of coke powder, 1-3 parts of graphite powder, 2-5 parts of potassium titanate, 2-4 parts of tire powder and 3-6 parts of zinc powder; The modified phenolic resin is prepared by the following steps: 1) Disperse molybdenum disulfide powder in water, add 3-mercapto-1,2-propylene glycol, disperse by ultrasonication for 2-6 hours, then react by mechanical stirring for 24-30 hours, filter, and obtain hydroxylated molybdenum disulfide; 2) Hexadecyltrimethoxysilane, polyvinylpyrrolidone, sodium dodecylbenzenesulfonate and water are added to a reaction vessel, stirred at 600-800 r / min for 40-60 min, and then an appropriate amount of triethylamine is added, and the stirring reaction is continued for 12-15 h. After the reaction is completed, the reaction product is centrifuged, filtered and washed to obtain polysiloxane microspheres; 3) Mix the phenol and formaldehyde dispersions uniformly, adjust the pH to 7.5-8 with ammonia water under stirring, heat to 70-80° C. and stir for reaction for 1.5-2 hours, then heat to 90-105° C. and continue stirring for reaction for 2-3 hours, then add the hydroxylated molybdenum disulfide obtained in step 1), 3-aminopropyltrimethoxysilane and polysiloxane microspheres obtained in step 2) in sequence, and stir for another 6-10 hours. After the reaction is completed, cool the reaction product to room temperature and filter it, wash the filter cake with anhydrous ethanol for 3-5 times, and dry it in a vacuum drying oven at 60-80° C. for 3-5 hours to obtain a modified phenolic resin; The basalt fiber is a modified basalt fiber, and the preparation method of the modified basalt fiber specifically comprises the following steps: (1) dissolving γ-aminopropyltriethoxysilane in a mixture of water and anhydrous ethanol, stirring for 10-20 minutes to mix them evenly, and obtaining a γ-aminopropyltriethoxysilane hydrolyzate; the volume ratio of water to anhydrous ethanol in the mixture of water and anhydrous ethanol is (2:8)-(3:7); (2) adding basalt fiber to the γ-aminopropyltriethoxysilane hydrolyzate obtained in step (1), stirring for 40-60 minutes to obtain a mixed solution 1, then adding a rare earth cerium chloride solution to the mixed solution 1, continuing to stir for 30-40 minutes, filtering, first naturally airing at room temperature for 20-30 hours, and then placing it in a vacuum drying oven at 100-120° C. for 1-2 hours to obtain modified basalt fiber; wherein the mass ratio of the basalt fiber, the γ-aminopropyltriethoxysilane hydrolyzate and the rare earth cerium chloride is 1:(3.5-6.5):(2-3); the mass percentage of the rare earth cerium chloride in the rare earth cerium chloride solution is 12-15%; and the mass percentage of the γ-aminopropyltriethoxysilane in the γ-aminopropyltriethoxysilane hydrolyzate is 0.9-1.5%.
2. The copper-free ceramic friction material for brake pads according to claim 1, characterized in that: In the step 1), the mass ratio of molybdenum disulfide powder, water and 3-mercapto-1,2-propylene glycol is (0.5-0.8):(50-400):(1.5-20).
3. The copper-free ceramic friction material for brake pads according to claim 1, characterized in that: In the step 2), the mass ratio of hexadecyltrimethoxysilane, polyvinylpyrrolidone, sodium dodecylbenzenesulfonate and water is (150-220):(0.8-2.5):(0.4-1):(600-900).
4. The copper-free ceramic friction material for brake pads according to claim 1, characterized in that: In the step 3), the molar ratio of phenol, formaldehyde, 3-aminopropyltrimethoxysilane and hydroxylated molybdenum disulfide is (0.8-1.2):(1.2-1.3):(0.1-0.15):(0.02-0.03).
5. The copper-free ceramic friction material for brake pads according to claim 1, characterized in that: The basalt fiber has a diameter of 3-8 μm and a length of 1-3.5 mm.
6. A method for preparing the copper-free ceramic friction material for brake pads as claimed in any one of claims 1 to 5, characterized in that: The steps include: Step S1, weighing each raw material according to the above weight parts; Step S2, placing the raw materials weighed in step S1 into a mixer according to corresponding weight portions and mixing them evenly to obtain a mixed raw material, wherein the main shaft speed of the mixer is 160-220 r / min, the reamer speed is 1900-2700 r / min, and the mixing time is 160-240 s; Step S3, pressing and heat treating the mixed raw materials obtained in step S2 in sequence to obtain the copper-free ceramic friction material for the brake pad.
7. The method for preparing a copper-free ceramic friction material for brake pads according to claim 6, characterized in that: The specific steps of pressing in step S3 are as follows: pressing the mixed raw materials through a hot press, the pressing temperature is 120-130°C, and the feeding amount is 195-200g each time; the pressing pressure is 40-50bar; the air is released after pressing for 2-4s, the air release time is 2-5s, and the air release is repeated 3 times, and the final pressure holding time is 160-180s, and the vacuum degree is 3-5bar.
8. The method for preparing a copper-free ceramic friction material for brake pads according to claim 6, characterized in that: The specific steps of the heat treatment in step S3 are as follows: first increase the temperature to 140-150°C, keep the temperature for 50-60 minutes, then increase the temperature to 150-160°C, keep the temperature for 60-70 minutes, then increase the temperature to 170-180°C, keep the temperature for 60-70 minutes, then increase the temperature to 190-200°C, keep the temperature for 120-140 minutes, and finally increase the temperature to 210-230°C, keep the temperature for 150-200 minutes, and the heating rate is 8-10 minutes / °C.