Environmentally friendly all-position welding electrode for pipeline steel and preparation method thereof

By preparing welding rods containing specific powder composition and lithium water glass adhesive, the problems of large dust generation and poor welding operation are solved in China's welding rods, and the welding effect of high strength, low diffusion hydrogen and low dust generation is achieved, which is suitable for 500 - Full position welding of 600MPa pipeline steel.

CN118287885BActive Publication Date: 2024-11-12INNER MONGOLIA ZHENGXIN CLOUD TECH SERVICE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410512298.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-11-12
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

Domestic alkaline welding rods produce a large amount of dust, especially in semi-enclosed environments, and there are few special welding rod manufacturers suitable for full-position welding, so the operability of vertical downward welding needs to be improved.

Method used

Prepare a full-position welding rod for environmentally friendly pipeline steel. The powder composition includes natural rutile, titanium dioxide, marble, microcrystalline fiber, fluorite, wollastonite, carboxymethyl cellulose, metal nickel, aluminum silver powder and iron powder , lithium water glass is added as the binder, and welding rods are prepared by dry mixing, wet stirring and multi-stage baking treatment to ensure high strength, low diffusion of the weld, and low dust generation.

Benefits of technology

It has achieved good welding performance of 500-600MPa pipeline steel, excellent impact toughness, low diffused hydrogen content, significantly reduced dust generation, and improved smoke toxicity. It is suitable for welding operations in semi-enclosed environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

An environmentally friendly all-position welding electrode for pipeline steel and a preparation method thereof, wherein the pipeline steel comprises pipeline steel with a tensile strength within the range of 500-600 MPa, the welding electrode comprises a welding core and a coating, the coating is prepared from powder and a binder, and the mass percentage of each component in the powder is as follows: natural rutile: 20-25%, titanium dioxide: 0-5%, electrolytic manganese: 3-8%, marble 25-30%, microcrystalline fiber: 5-10%, fluorite: 8-12%, wollastonite 5-10%, carboxymethyl cellulose: 0-2%, metallic nickel: 0.5-2%, aluminum silver powder 0-2%, and iron powder 10-20%; in the process of preparing the coating, the amount of the binder added is 13-17% of the total weight of the powder. The physical and chemical properties of this welding rod can meet the performance requirements of 500-600MPa pipeline steel, with excellent impact toughness, low diffusible hydrogen content, and significantly lower dust generation and smoke toxicity than existing technologies. It has excellent environmental performance and can effectively improve the smoke generation and toxicity in semi-closed working environments during pipeline welding and repair.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an environmentally friendly all-position welding electrode for pipeline steel and a preparation method thereof, belonging to the technical field of welding materials. Background Art

[0002] Pipeline steel (HSLA) with excellent comprehensive performance obtained through controlled rolling and controlled cooling technology is widely used in petrochemical and natural gas transportation projects. During use, it is often encountered on-site welding or repair, and workers are required to perform full-position welding operations in a semi-enclosed environment. In order to meet the high requirements of pipeline steel welds for diffusible hydrogen content, basic electrodes are used as much as possible, but the dust generation of domestic basic electrodes has been a technical problem for many years, especially for workers working in semi-enclosed environments. In addition, at present, only a few welding rod factories in China can produce special welding rods suitable for full-position welding, but the slag system is mostly acidic slag system, and the full-position welding process performance, especially the operability of vertical downward welding, still needs to be improved. Summary of the invention

[0003] The purpose of the present invention is to provide an environmentally friendly all-position welding electrode for pipeline steel and a preparation method thereof. The physical and chemical properties of the electrode can meet the performance requirements of 500-600MPa pipeline steel, and the electrode has excellent impact toughness and low diffusible hydrogen content.

[0004] The technical scheme adopted by the present invention to achieve its invention purpose is: an environmentally friendly all-position welding electrode for pipeline steel and a preparation method thereof, wherein the pipeline steel includes pipeline steel with a tensile strength within the range of 500-600MPa, the welding electrode includes a welding core and a coating, the coating is prepared from powder and a binder, and the mass percentage of each component in the powder is as follows: natural rutile: 20-25%, titanium dioxide: 0-5%, electrolytic manganese: 3-8%, marble 25-30%, microcrystalline fiber: 5-10%, fluorite: 8-12%, wollastonite 5-10%, carboxymethyl cellulose: 0-2%, metallic nickel: 0.5-2%, aluminum silver powder 0-2%, iron powder 10-20%; in the process of preparing the coating, the amount of the binder added is 13-17% of the total weight of the powder.

[0005] Furthermore, the pipeline steel described in the present invention includes petroleum and natural gas steel pipes with models L390 or X56, L415 or X60, L450 or X65 in GB / T9711-2017.

[0006] Furthermore, the mass percentages of the components in the medicinal powder of the present invention are as follows: natural rutile: 22-25%, titanium dioxide: 0-2%, electrolytic manganese: 5-8%, marble 26-29%, microcrystalline fiber: 5-8%, fluorite: 9-11%, wollastonite 6-9%, carboxymethyl cellulose: 0.5-1.2%, metallic nickel: 0.8-1.5%, aluminum silver powder 0.5-1.5%, iron powder 12-16%. In the process of preparing the medicinal coating, the amount of the binder added is 14-16% of the total weight of the medicinal powder.

[0007] Further, the particle size distribution of each component in the medicinal powder of the present invention is as follows: the particle size of natural rutile is 60-140 mesh, the particle size of titanium dioxide is 200-325 mesh, the particle size of electrolytic manganese is 60-160 mesh, the particle size of marble is 60-160 mesh, the particle size of microcrystalline fiber is 200-400 mesh, the particle size of fluorite is 60-160 mesh, the particle size of wollastonite is 60-160 mesh, the particle size of carboxymethyl cellulose is 80-160 mesh, the particle size of metallic nickel is 80-160 mesh, the particle size of aluminum silver powder is 100-150 mesh, and the particle size of iron powder is 100-150 mesh.

[0008] Furthermore, the ratio of the coating weight to the welding core weight of the present invention is 28±2%.

[0009] Furthermore, the binder of the present invention is lithium water glass.

[0010] Furthermore, the total amount of marble and fluorite described in the present invention accounts for 35-40% of the total weight of the medicine powder, and the total amount of the aluminosilicate and titanate accounts for 30-35% of the total weight of the medicine powder. The aluminosilicate includes aluminosilicate generated by the metallurgical reaction of wollastonite, lithium water glass, and aluminum silver powder in the molten pool; the titanate includes titanate generated by the metallurgical reaction of rutile and titanium dioxide in the molten pool.

[0011] The preparation method of the above-mentioned environmentally friendly all-position welding electrode for pipeline steel comprises the following steps: dry-mixing the components of the powder, then adding a binder and wet-stirring to obtain a mixed powder, using a special welding rod production hydraulic press to evenly press the mixed powder onto the surface of the welding core to obtain a welding rod, and performing low-temperature baking, medium-temperature baking, and high-temperature baking in sequence, and obtaining the environmentally friendly all-position welding electrode for pipeline steel after natural cooling.

[0012] Furthermore, the coating pressure of the oil hydraulic press for preparing the welding rod in the preparation method of the present invention is 20-30MPa.

[0013] Furthermore, the low-temperature baking temperature of the preparation method of the present invention is 60-80°C, and the time is 1-2h; the medium-temperature baking temperature is 80-120°C, and the time is 0.5-1h; the high-temperature baking temperature is 180-200°C, and the time is 0.5-1.5h.

[0014] The mechanism of action and limiting principle of each component in the welding electrode coating of the present invention are as follows:

[0015] Natural rutile: Natural rutile has weak oxidizability, good thermal slag removal properties, stabilizes the arc, allows the metal to transition in a fine mist, adjusts the viscosity and surface tension of the slag, forms ultra-short slag, and ensures that the molten pool solidifies in a shorter time during all-position welding. When the content is less than 20%, the improvement effect on all-position welding is not significant. When the content is higher than 25%, the viscosity of the liquid molten pool increases and the fluidity deteriorates, which is not conducive to weld formation.

[0016] The crystal structure and melting point of titanium dioxide are somewhat different from those of natural rutile, which can form short slag in a wider temperature range to ensure the feasibility of all-position welding. Combined with CMC (carboxymethyl cellulose), it can improve the pressure coating performance, and its range is limited to 0-5%. When the content is greater than 5%, the cost increases compared with natural rutile.

[0017] Electrolytic manganese (Mn ≥ 99.8%) undergoes a substitution reaction to desulfurize and deoxidize, and transfers Mn elements to the weld to improve the strength and crack resistance of the weld. The range is limited to 3-8%. When the content is lower than 3%, deoxidation is insufficient, and the Mn element cannot be transferred to the weld metal, and the weld strength is reduced; when the content is higher than 8%, the weld strength is significantly improved, which is not suitable for welding steel pipes of the matching strength level of the present invention, and the cost is increased.

[0018] Marble (CaCO3≥98%) is mainly used for slag and gasification, protecting the weld from oxidation and nitridation by air, and can adjust the melting point, viscosity, surface tension and interfacial tension of the slag. Its content is limited to 25-30%. When the content is less than 25%, the slag is insufficient and the weld formation cannot be guaranteed; when the content is greater than 30%, it violates the original intention of environmentally friendly welding rods and is not conducive to the realization of all-position welding (especially vertical downward welding).

[0019] The main component of microcrystalline fiber is cotton or wood fiber, with a carbonization point of 280℃, low moisture content, and heat resistance of >150℃. Its main function is to ensure sufficient blowing force and stiffness of the arc during full-position operation. When the content is less than 5%, the force is slightly insufficient, especially during vertical 90° downward operation. When the content is greater than 10%, it affects the stability of the arc and leads to increased welding spatter. At the same time, special pretreatment is carried out before use to improve its heat resistance.

[0020] Fluorite (CaF2≥96%) reduces the surface tension of liquid metal, improves fluidity, and reduces weld porosity sensitivity and diffusible hydrogen content of deposited metal. Because the generated fluoride causes a sharp increase in the amount of dust generated by the electrode, the present invention limits the amount of fluorite added to 8-12%. When the content is lower than 8%, the slag becomes weakly acidic, resulting in an increase in the diffusible hydrogen content of the weld and a decrease in the toughness of the weld; when the content is higher than 12%, the amount of dust generated increases sharply, which violates the original intention of the design of an environmentally friendly electrode.

[0021] Wollastonite is a natural calcium metasilicate mineral with the molecular formula of CaSiO3. It has physical properties such as a small linear expansion coefficient and a narrow crystal phase transition temperature range. At the same time, it can increase the permeability of the slag, making up for the fact that the diffusible hydrogen content of the deposited metal caused by the reduction of fluorite does not meet the national standard requirements. According to experimental demonstration, silicon and alkali metals and alkaline earth metals can form a glassy state and enter the slag. Increasing silicates in the coating can not only reduce smoke, but also reduce the toxicity of smoke due to the combination with alkali metals and alkaline earth metals in the arc atmosphere. The present invention limits its content to 5-10%. When the content is lower than 5%, the effect of reducing the amount of smoke and the toxicity of smoke is not obvious. When the content is higher than 10%, the slag removal performance is affected, and it is not conducive to the full-position welding of the electrode.

[0022] The main function of carboxymethyl cellulose is to increase slip, improve the pressure coating performance of the welding rod, and has a certain gas-generating function, which makes up for the insufficient blowing force of the microcrystalline fiber caused by burning at the high temperature stage. The present invention limits its range to 0-2%. If it is not added, the pressure coating effect is reduced. If the content is higher than 2%, the manufacturing cost is increased.

[0023] Metallic nickel can improve the toughness of the ferrite matrix and promote the formation of acicular ferrite, improve the crack resistance of the weld, and enhance the low-temperature impact toughness. The addition amount in the present invention is 0.5-2%. When the content is less than 0.5%, the ability to improve the toughness of the weld metal is insufficient, and when the content is higher than 2%, the manufacturing cost is increased.

[0024] Aluminum silver powder undergoes substitution reaction deoxidation to form high melting point Al2O3, which regulates the melting point and solidification temperature of the slag. Ensure the appropriate sleeve length during electrode welding, so that the arc forms a more directional and concentrated high-speed airflow, obtain greater arc blowing force and stiffness, and can act as a non-spontaneous nucleation particle to solidify the slag as early as possible, thereby ensuring the realization of the full-position welding process. The present invention limits its range to 0-2%. When the content is higher than 2%, too much high melting point material is formed, affecting the fluidity of the molten pool. At the same time, the high melting point material has a limited effect on the sleeve length. Too much will coarsen the molten droplet and reduce the melting speed of the welding core.

[0025] Iron powder (Fe≥99%) can improve the welding efficiency of the electrode, reduce the ionization potential of the arc space, and improve the arc stability; reduce the slag coefficient, which is beneficial to improve the process performance of the electrode, reduce spatter, make the forming smooth, and make the slag removal easy. The present invention limits its range to 10-20%. When the content is less than 10%, the improvement of welding process performance is not significant. When the content is greater than 20%, the amount of weld slag is significantly reduced and the weld formation is deteriorated.

[0026] The binder is industrially produced with lithium water glass, which has more stable performance. The product has stronger performance stability and can be used directly without re-baking during use. It greatly reduces the difficulty of field construction. The range is limited to 13-17%. If the content is lower than 13%, the pressure coating effect is poor and the strength of the electrode coating is insufficient. If the content is higher than 17%, the total amount of silicate in the molten pool increases, resulting in poor operability in all positions and increased dust generation of the electrode.

[0027] Compared with the prior art, the beneficial effects of the present invention are:

[0028] The welding rod of the present invention can be used for all-position welding of pipeline steel with a tensile strength within the range of 500-600MPa, has excellent impact toughness, low diffusible hydrogen content, and the amount of dust and smoke toxicity are significantly lower than those of the prior art. The amount of dust is reduced from about 12g / kg to about 7g / kg on the basis of current pipeline steel welding rods, and the soluble fluorine content is reduced from 15% to about 11%. It has excellent environmental protection performance and can effectively improve the amount of smoke and toxicity in a semi-closed working environment during pipeline welding and repair. DETAILED DESCRIPTION Example

[0029] An environmentally friendly all-position welding electrode for pipeline steel and a preparation method thereof. The pipeline steel includes pipeline steel with a tensile strength within the range of 500-600 MPa. The welding electrode includes a welding core and a coating. The coating is prepared from powder and a binder. The mass percentage of each component in the powder is as follows: natural rutile: 20-25%, titanium dioxide: 0-5%, electrolytic manganese: 3-8%, marble 25-30%, microcrystalline fiber: 5-10%, fluorite: 8-12%, wollastonite 5-10%, carboxymethyl cellulose: 0-2%, metallic nickel: 0.5-2%, aluminum silver powder 0-2%, and iron powder 10-20%. In the process of preparing the coating, the amount of binder added is 13-17% of the total weight of the powder.

[0030] Preferably, the pipeline steel includes petroleum and natural gas steel pipes with models L390 or X56, L415 or X60, L450 or X65 in GB / T9711-2017.

[0031] Preferably, the mass percentage of each component in the medicine powder is as follows: natural rutile: 22-25%, titanium dioxide: 0-2%, electrolytic manganese: 5-8%, marble 26-29%, microcrystalline fiber: 5-8%, fluorite: 9-11%, wollastonite 6-9%, carboxymethyl cellulose: 0.5-1.2%, metallic nickel: 0.8-1.5%, aluminum silver powder 0.5-1.5%, iron powder 12-16%. In the process of preparing the medicine coating, the amount of binder added is 14-16% of the total weight of the medicine powder.

[0032] Preferably, the particle size distribution of each component in the medicinal powder is as follows: the particle size of natural rutile is 60-140 mesh, the particle size of titanium dioxide is 200-325 mesh, the particle size of electrolytic manganese is 60-160 mesh, the particle size of marble is 60-160 mesh, the particle size of microcrystalline fiber is 200-400 mesh, the particle size of fluorite is 60-160 mesh, the particle size of wollastonite is 60-160 mesh, the particle size of carboxymethyl cellulose is 80-160 mesh, the particle size of metallic nickel is 80-160 mesh, the particle size of aluminum silver powder is 100-150 mesh, and the particle size of iron powder is 100-150 mesh.

[0033] Preferably, the ratio of the coating weight to the welding core weight is 28±2%.

[0034] Preferably, the binder is lithium water glass.

[0035] Preferably, the total amount of the marble and fluorite accounts for 35-40% of the total weight of the medicine powder, and the total amount of the aluminosilicate and titanate accounts for 30-35% of the total weight of the medicine powder. The aluminosilicate includes aluminosilicate generated by the metallurgical reaction of wollastonite, lithium water glass, and aluminum silver powder in the molten pool; the titanate includes titanate generated by the metallurgical reaction of rutile and titanium dioxide in the molten pool.

[0036] The preparation method of the environment-friendly all-position welding electrode for pipeline steel of the present invention comprises the following steps: dry-mixing the components of the powder, adding a binder and wet-stirring the mixture to obtain a mixed powder, applying the mixed powder evenly on the surface of the welding core by a special welding rod production hydraulic press to obtain a welding rod, and sequentially performing low-temperature baking, medium-temperature baking and high-temperature baking to obtain the environment-friendly all-position welding electrode for pipeline steel after natural cooling.

[0037] Preferably, the coating pressure of the oil hydraulic press used in the preparation method for preparing the welding rod is 20-30 MPa.

[0038] Preferably, the low-temperature baking temperature in the preparation method is 60-80°C, and the time is 1-2h; the medium-temperature baking temperature is 80-120°C, and the time is 0.5-1h; the high-temperature baking temperature is 180-200°C, and the time is 0.5-1.5h.

[0039] The following examples illustrate the implementation methods and technical effects of the present invention. Table 1 shows the mass percentage of each component in the powder of four specific embodiments. The particle size of the powder of the four embodiments adopts the particle size distribution limited as above. The preparation method of the welding rod is as follows: dry-mix the components of the powder, then add a binder and wet-mix to obtain a mixed powder, use a special welding rod production hydraulic press to evenly press the mixed powder on the surface of the welding core to obtain a welding rod, and then perform low-temperature baking, medium-temperature baking, and high-temperature baking in sequence, and obtain the environmentally friendly welding rod for all-position welding of pipeline steel after natural cooling. The specific preparation parameters are shown in Table 2.

[0040] The deposited metal performance test of the prepared welding rod was carried out by manual arc method. The experimental parameters are shown in Table 3.

[0041] The chemical composition of the deposited metal of the welding rods prepared in Examples 1-4 was analyzed, the mechanical properties were tested, and the diffusible hydrogen content was tested. The results are shown in Table 4, Table 5, and Table 6, respectively.

[0042] Table 1 Composition and proportion of welding rod powder in the embodiment of the present invention (mass percentage)

[0043]

[0044] Table 2 Preparation parameters of welding rods according to the present invention

[0045]

[0046] Table 3 Deposited metal welding parameters

[0047]

[0048] Table 4 Chemical composition of the cladding metal of the welding rod in the embodiment of the present invention (mass percentage %)

[0049]

[0050] Table 5 Mechanical properties of the cladding metal of the welding rod in the embodiment of the present invention

[0051]

[0052] Table 6 Diffusible hydrogen content of the cladding metal of the welding rod in the embodiment of the present invention

[0053]

[0054] A statistical experiment on the dust generation of the welding rods prepared in Examples 1-4 was conducted (the comparison product was a special welding rod for pipeline steel of the same strength level produced by a welding material factory). The results are shown in Table 7.

[0055] Table 7 Experimental results of dust generation of welding rods of the embodiments of the present invention and comparative products

[0056]

[0057] The welding rods prepared in Examples 1-4 were subjected to statistical experiments on the soluble fluorine content (the comparative product was a special welding rod for basic pipeline steel of the same strength produced by a welding material factory). The results are shown in Table 8.

[0058] Table 8 Experimental results of soluble fluorine content in welding of the embodiments of the present invention and comparative products

[0059]

[0060] The experimental test results of the mechanical properties of the weld metal show that the physical and chemical properties of the product meet the performance requirements of 500-600MPa pipeline steel, with excellent impact toughness and low diffusible hydrogen content. The dust emission of the welding rod has been reduced from about 12g / kg to about 7g / kg based on the original pipeline steel welding rod, and the soluble fluorine content has been reduced from 15% to about 11%. The welding process is good in all positions, especially vertical downward, and baking-free welding can be performed in field construction, providing high-quality welding materials for field construction of pipeline steel.

Claims

1. An environmentally friendly all-position welding electrode for pipeline steel, characterized by: The pipeline steel has a tensile strength within the range of 500-600 MPa. The welding rod comprises a welding core and a coating. The coating is prepared from powder and a binder. The mass percentage of each component in the powder is as follows: natural rutile: 20-25%, titanium dioxide: 0-5%, electrolytic manganese: 3-8%, marble 25-30%, microcrystalline fiber: 5-10%, fluorite: 8-12%, wollastonite 5-10%, carboxymethyl cellulose: 0-2%, metallic nickel: 0.5-2%, aluminum silver powder 0-2%, and iron powder 10-20%. In the process of preparing the coating, the amount of binder added is 13-17% of the total weight of the powder.

2. The environmentally friendly all-position welding electrode for pipeline steel according to claim 1, characterized in that: The pipeline steel includes petroleum and natural gas steel pipes with models L390 / X56, L415 / X60, and L450 / X65 in GB / T9711-2017.

3. The environmentally friendly all-position welding electrode for pipeline steel according to claim 1, characterized in that: The mass percentages of the components in the medicine powder are as follows: natural rutile: 22-25%, titanium dioxide: 0-2%, electrolytic manganese: 5-8%, marble 26-29%, microcrystalline fiber: 5-8%, fluorite: 9-11%, wollastonite 6-9%, carboxymethyl cellulose: 0.5-1.2%, metallic nickel: 0.8-1.5%, aluminum silver powder 0.5-1.5%, iron powder 12-16%. In the process of preparing the medicine coating, the amount of binder added is 14-16% of the total weight of the medicine powder.

4. The environmentally friendly all-position welding electrode for pipeline steel according to claim 1, characterized in that: The particle size distribution of each component in the medicinal powder is as follows: the particle size of natural rutile is 60-140 meshes, the particle size of titanium dioxide is 200-325 meshes, the particle size of electrolytic manganese is 60-160 meshes, the particle size of marble is 60-160 meshes, the particle size of microcrystalline fiber is 200-400 meshes, the particle size of fluorite is 60-160 meshes, the particle size of wollastonite is 60-160 meshes, the particle size of carboxymethyl cellulose is 80-160 meshes, the particle size of metallic nickel is 80-160 meshes, the particle size of aluminum silver powder is 100-150 meshes, and the particle size of iron powder is 100-150 meshes.

5. The environmentally friendly all-position welding electrode for pipeline steel according to claim 1, characterized in that: The ratio of the coating weight to the welding core weight is 28±2%.

6. The environmentally friendly all-position welding electrode for pipeline steel according to claim 1, characterized in that: The binder is lithium water glass.

7. The environmentally friendly all-position welding electrode for pipeline steel according to claim 6, characterized in that: The total amount of marble and fluorite accounts for 35-40% of the total weight of the medicine powder, wollastonite, lithium water glass, and aluminum silver powder participate in the metallurgical reaction of the molten pool to generate aluminosilicate, rutile and titanium dioxide participate in the metallurgical reaction of the molten pool to generate titanate, and the total amount of aluminosilicate and titanate accounts for 30-35% of the total weight of the medicine powder.

8. A method for preparing an environment-friendly all-position welding electrode for pipeline steel according to any one of claims 1 to 7, comprising the following steps: dry-mixing the components of the powder, then adding a binder and wet-stirring to obtain a mixed powder, using a special welding rod production hydraulic press to evenly press the mixed powder onto the surface of the welding core to obtain a welding rod, and sequentially performing low-temperature baking, medium-temperature baking, and high-temperature baking to obtain the environment-friendly all-position welding electrode for pipeline steel after natural cooling.

9. The method for preparing the environmentally friendly all-position welding electrode for pipeline steel according to claim 8, characterized in that: The pressure of the oil press for preparing welding rods is 20-30MPa.

10. The method for preparing the environmentally friendly all-position welding electrode for pipeline steel according to claim 8, characterized in that: The low-temperature baking temperature is 60-80°C and the time is 1-2h; the medium-temperature baking temperature is 80-120°C and the time is 0.5-1h; the high-temperature baking temperature is 180-200°C and the time is 0.5-1.5h.