A method for preparing a self-cleaning agricultural anti-fog shed film
By using a combination of methyl methacrylate, polydimethylsiloxane and nano-silica microcapsules on the agricultural shed film, the problem of insufficient hydrophobicity and anti-fog performance of the shed film is solved, and self-healing and efficient are achieved Waterproof effect, extending service life and promoting crop growth.
Patent Information
- Application Number
- CN202410713981.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-04
AI Technical Summary
Existing agricultural shed films have poor hydrophobicity and poor anti-fog performance, and the coating cannot heal itself or has a long self-healing period after being damaged, which affects crop growth and service life.
Using ingredients such as methyl methacrylate, polydimethylsiloxane and nano-silica microcapsules, a hydrophobic coating is prepared through spin coating technology, and the self-healing mechanism of nano-silica microcapsules is utilized under UV light irradiation. , restore hydrophobic properties.
Significantly improve the hydrophobic performance and durability of the shed membrane, ensure the stability of the waterproof effect in long-term use, avoid the accumulation of water mist, promote photosynthesis, extend the service life, and reduce energy loss.
Abstract
Description
Technical Field
[0001] The present application belongs to the field of composite materials, and specifically relates to a method for preparing a self-cleaning agricultural anti-fog shed film. Background Art
[0002] As a facility widely used in agricultural production, polyethylene plastic sheds have many advantages. Polyethylene plastic sheds are made of high-density polyethylene materials and have good thermal insulation properties. In winter, the temperature in the shed can be maintained within a relatively stable range, providing a suitable environment for crop growth. At the same time, on sunny days, the temperature in the shed can also rise rapidly, promoting crop growth. This thermal insulation performance gives polyethylene plastic sheds great advantages in agricultural production. The light transmittance of polyethylene plastic sheds is relatively high, usually reaching more than 80%. This high light transmittance allows sufficient light in the shed, which is conducive to the photosynthesis and growth and development of crops. At the same time, high light transmittance can also increase the temperature in the shed, further promoting crop growth. Polyethylene plastic sheds have good corrosion resistance and can resist the erosion of chemicals such as acids and alkalis. This corrosion resistance makes the shed film less susceptible to damage during use and extends its service life. In addition, polyethylene plastic sheds also have good anti-aging properties and can maintain good physical properties during long-term use. The structure of polyethylene plastic sheds is relatively simple, easy to build, and does not require the use of a large amount of building materials. At the same time, the shed film itself is light and easy to transport and install. This lightweight structure makes polyethylene plastic sheds very flexible in agricultural production and can be built and dismantled at any time as needed. The investment cost of polyethylene plastic sheds is relatively low, and they have a long service life and low maintenance costs. At the same time, because the environment in the shed is suitable for crop growth, it can improve the yield and quality of crops, thereby bringing significant economic benefits. In addition, polyethylene plastic sheds can also reduce the use of pesticides and fertilizers, reducing agricultural production costs.
[0003] However, there are also some problems in the use of greenhouses or sheds, especially in environments with high humidity, where droplets are prone to appear on the inner surface of polyethylene plastic sheds. These droplets will not only affect the photosynthesis of crops, but also hinder the ventilation effect in the shed, thereby affecting the growth and yield of crops. When polyethylene plastic sheds encounter rain or dew, water droplets are likely to form on the surface instead of sliding off quickly. This will not only increase the humidity in the shed, but may also affect the growth environment of crops. It may be that the surface energy of polyethylene materials is relatively high, making it easy for water molecules to form a stable contact angle on its surface, leading to the formation of water droplets. In addition, the wetting properties of the polyethylene material itself are also poor, that is, the water droplets have a strong adhesion to the surface and are difficult to slide off. Therefore, many scholars have tried to modify the polyethylene shed film in the hope of obtaining a shed film with good hydrophobic and anti-fog properties and that can achieve self-cleaning properties.
[0004] At present, the method for improving the hydrophobicity of polyethylene materials is mainly through coating the surface or performing nanostructure treatment on the surface of the product, thereby making the material more hydrophobic.
[0005] The patent with the announcement number CN114644773B discloses a method for preparing an antifreeze self-cleaning agricultural anti-fog shed film, which specifically includes adding N,N-dimethylformamide, acetic acid and n-octyltriethoxysilane to tetrabutyl titanate to prepare reaction solution A, adding corn protein and sodium dodecyl sulfate to deionized water and sequentially adding gelatin, glucose, polyethylene glycol and nano-silicon dioxide to prepare reaction solution B, and then spin-coating the reaction solutions A and B on a blown polyethylene shed and drying them to obtain a polyethylene shed film with a durable anti-fog performance. The patent with the announcement number CN102744943B discloses a method for manufacturing a high-performance polyolefin coated agricultural film. Through a special coating process, it changes the status quo of the 3-6-month dripping period of the traditional dripping film and achieves the effect of extending the dripping time. However, the designs of these two patents face a significant challenge in the long-term use process. Once the coating is damaged, it will not be able to automatically repair, which may have a negative impact on the overall anti-fog performance and service life of the shed film.
[0006] The patent with announcement number CN117986939A discloses an anti-fog shed film coating liquid, an agricultural anti-fog shed film, and a preparation method and application thereof. The anti-fog shed film coating liquid contains a solvent and a film-forming agent; wherein the film-forming agent contains polyvinyl alcohol and alginate, which have good film-forming properties and low price. The prepared film layer has long-lasting anti-fog properties and has certain wear resistance and self-healing properties. However, the self-healing property of the anti-fog coating of this application relies on the fact that the water molecules adsorbed in the coating can interact with the hydroxyl or carboxyl groups of PVA and SA to rebuild broken hydrogen bonds. It has a high degree of dependence on the humidity of the environment, and during the self-healing process, some chemical bonds may not be fully restored, resulting in gradual destruction of the coating structure and degradation of performance.
[0007] To sum up, in view of the problems existing in the prior art, such as poor hydrophobicity of agricultural greenhouse films, poor anti-fog performance, and the inability of the greenhouse films to self-heal after being damaged or a long self-healing period, it is urgent to propose a self-cleaning agricultural anti-fog greenhouse film to alleviate the current problems. Summary of the invention
[0008] In view of the problems existing in the prior art such as poor hydrophobicity and anti-fog performance of agricultural greenhouse films, the inability of the films to self-heal after being damaged or a long self-healing period, the present application proposes a method for preparing a self-cleaning agricultural anti-fog greenhouse film.
[0009] The technical solution of this application:
[0010] A method for preparing a self-cleaning agricultural anti-fog shed film comprises the following steps:
[0011] Step S1. Methyl methacrylate, polydimethylsiloxane, a silane coupling agent, azobisisobutyronitrile and ethyl acetate are mixed and stirred to obtain a mixed solution A;
[0012] Step S2. Methanol is added to the mixed solution A, the obtained precipitate is washed with a detergent, and vacuum dried to obtain a solid sample;
[0013] Step S3. Add the nano-silicon dioxide suspension to the solid sample obtained in step S2 and mix them to obtain a mixed solution B for standby use;
[0014] Step S4. Mixing and inflating a silane coupling agent, high-density polyethylene, pentaerythritol tetra(bis-T-butylhydroxyhydrocinnamate) ester and nano-silica microcapsules to obtain a plastic film;
[0015] Step S5. Spin-coat the mixed solution B obtained in step S3 onto the surface of step S4 to obtain a self-cleaning agricultural anti-fog shed film.
[0016] In a specific implementation scheme, the mass ratio of methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate in step S1 is (50~70):(60~80):(10~20):1:(140~160), the reaction temperature is 70~80°C, the stirring time is 10~12h, and the stirring reaction needs to be completed in a nitrogen atmosphere.
[0017] In a specific implementation scheme, the mass ratio of methanol to mixed liquid A in step S2 is 1:(60-80), the detergent is ethyl alcohol, the washing times are 2-3 times, the vacuum drying temperature is 40-60°C, and the vacuum drying time is 12-15h.
[0018] In a specific implementation scheme, the mass fraction of the nano-silica suspension in step S3 is 1%, the mass ratio of the solid sample to the nano-silica suspension is 1:(50-100), and the mixing treatment is ultrasonic treatment at room temperature for 20-30 minutes, followed by stirring for 30-60 minutes.
[0019] In a specific implementation scheme, the mass ratio of high-density polyethylene, silane coupling agent, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and nano-silica microcapsules in step S4 is (80-90):(3-5):(1-3):(2-4), and the inflation adopts multi-stage temperature control, wherein the temperature of the feeding section is controlled at 60-100°C, the temperature of the melt mixing section is controlled at 100-120°C, the temperature of the metering section is controlled at 150-170°C, and the temperature of the die head is controlled at 150-180°C.
[0020] By adopting the above technical solution, the hydrophobic coating combines methyl methacrylate and polydimethylsiloxane, each of which brings unique performance advantages to the coating. The hydrophobicity of methyl methacrylate is mainly due to the methyl group in its molecular structure, which can significantly reduce the interaction between the coating and water molecules, thereby greatly improving the waterproof performance of the coating. The addition of polydimethylsiloxane further enhances the hydrophobicity and weather resistance of the coating. The siloxane bond in the molecular structure of polydimethylsiloxane is the key to its strong hydrophobicity. This bond structure makes it difficult for water molecules to form a stable attachment on the surface of the coating, thereby ensuring the efficient waterproof performance of the coating. At the same time, polydimethylsiloxane also has excellent weather resistance and can maintain stable performance under high or low temperature conditions, which enables the hydrophobic coating to maintain excellent waterproof effect in various extreme environments, greatly improving the service life and durability of the coating.
[0021] In a specific embodiment, the preparation method of the nano-silicon dioxide microcapsules in step S4 is:
[0022] Step S41. reacting polyethylene glycol octylphenyl ether, isocyanate propyltriethoxysilane and dibutyltin dilaurate to obtain a mixed reaction system 1;
[0023] Step S42. Add nano-silicon dioxide to the mixed reaction system 1, adjust the pH value to 7-9, and react to obtain a mixed reaction system 2;
[0024] Step S43: Deoxygenate the mixed reaction system 2 with nitrogen, continue the reaction, and obtain a mixed reaction system 3. Then separate the solid and the liquid, and dry the obtained solid to obtain nano-silica microcapsules.
[0025] In a specific implementation scheme, the mass ratio of polyethylene glycol octylphenyl ether, isocyanate propyltriethoxysilane, dibutyltin dilaurate and nano-silicon dioxide is (3~5):(0.8~1.2):(0.8~1.2):1; the reaction conditions in step S41 are stirring at 40~60°C for 16~24h; the reaction conditions in step S42 are stirring at 55~75°C for 20~28h, and the reaction conditions in step S43 are stirring at 60~80°C for 20~28h.
[0026] By adopting the above technical scheme, nano-silica microcapsules are added to the greenhouse film preparation material, which not only enhances the hydrophobic properties of the greenhouse film, but also gives it the ability to self-repair. In agricultural production, when the hydrophobic coating surface of the greenhouse film is etched, mechanically damaged or oil-contaminated, the hydrophobic properties are reduced, which in turn affects the photosynthesis of the plant and the service life of the greenhouse film. By introducing nano-silica microcapsules with ultraviolet light response characteristics, when the hydrophobic coating on the surface of the greenhouse film is damaged, under ultraviolet light irradiation, nano-silica can catalyze the decomposition of the polymer on the surface of the microcapsule, causing the microcapsule to swell. The released molecules can quickly fill the defects on the coating surface, self-repair, and restore its hydrophobic properties. This self-repair mechanism not only improves the durability of the greenhouse film, but also ensures that the greenhouse film always maintains good hydrophobic properties during long-term use. In addition, the synergistic effect of nano-silica microcapsules and the hydrophobic layer on the surface of the greenhouse film, the greenhouse film in this application can more effectively avoid the accumulation of water mist on the surface, thereby ensuring that the plant obtains sufficient light and promotes photosynthesis. It greatly facilitates agricultural production and provides a strong guarantee for the healthy growth of crops. In this application, nano-silicon dioxide is added to both the hydrophobic coating and the greenhouse film. Its porous structure is conducive to improving the air permeability of the material, avoiding excessive moisture and moisture resistance, thereby improving the durability of the coating; due to its high surface area and special surface activity, nano-silicon dioxide particles can form a strong interaction force with other polymer molecules and form a network structure in the polymer matrix, thereby significantly improving the mechanical strength and hardness of the polymer; in addition, nano-silicon dioxide can significantly improve the material's resistance to ultraviolet aging and extend the material's service life; at the same time, nano-silicon dioxide has good thermal insulation properties, which can effectively prevent heat transfer, thereby reducing energy loss and achieving efficient thermal insulation effects.
[0027] Beneficial effects of this application:
[0028] (1) In the present application, the hydrophobic coating incorporates methyl methacrylate and polydimethylsiloxane, each of which brings unique performance advantages to the coating. The hydrophobicity of methyl methacrylate is mainly due to the methyl group in its molecular structure, which can significantly reduce the interaction between the coating and water molecules, thereby greatly improving the waterproof performance of the coating. The addition of polydimethylsiloxane further enhances the hydrophobicity and weather resistance of the coating. The siloxane bond in the molecular structure of polydimethylsiloxane is the key to its strong hydrophobicity. This bond structure makes it difficult for water molecules to form a stable attachment on the surface of the coating, thereby ensuring the efficient waterproof performance of the coating. At the same time, polydimethylsiloxane also has excellent weather resistance and can maintain stable performance under high or low temperature conditions, which enables the hydrophobic coating to maintain excellent waterproof effect in various extreme environments, greatly improving the service life and durability of the coating.
[0029] (2) The present application adds nano-silica microcapsules to the greenhouse film preparation material, which not only enhances the hydrophobic properties of the greenhouse film, but also gives it the ability to self-repair. In agricultural production, when the hydrophobic coating on the surface of the greenhouse film is etched, mechanically damaged or contaminated with oil, the hydrophobic properties will decrease, which will in turn affect the photosynthesis of the plants and the service life of the greenhouse film. By introducing nano-silica microcapsules with ultraviolet light response characteristics, when the hydrophobic coating on the surface of the greenhouse film is damaged, under ultraviolet light irradiation, nano-silica can catalyze the decomposition of the polymer on the surface of the microcapsules, causing the microcapsules to swell. The released molecules can quickly fill the defects on the coating surface, self-repair, and restore its hydrophobic properties. This self-repair mechanism not only improves the durability of the greenhouse film, but also ensures that the greenhouse film always maintains good hydrophobic properties during long-term use. In addition, the synergistic effect of nano-silica microcapsules and the hydrophobic layer on the surface of the greenhouse film, the greenhouse film in the present application can more effectively prevent water mist from gathering on the surface, thereby ensuring that the plants obtain sufficient light and promoting photosynthesis. It greatly facilitates agricultural production and provides strong guarantee for the healthy growth of crops.
[0030] (3) In the present application, nano-silica is added to both the hydrophobic coating and the greenhouse film raw materials. Its porous structure is conducive to improving the air permeability of the material, avoiding excessive moisture and moisture resistance, thereby improving the durability of the coating; due to its high surface area and special surface activity, nano-silica particles can form a strong interaction force with other polymer molecules and form a network structure in the polymer matrix, thereby significantly improving the mechanical strength and hardness of the polymer; in addition, nano-silica can significantly improve the material's resistance to ultraviolet aging and extend the material's service life; at the same time, nano-silica has good thermal insulation properties and can effectively prevent heat transfer, thereby reducing energy loss and achieving efficient thermal insulation effects. DETAILED DESCRIPTION
[0031] In order to further explain the technical means and effects adopted by the present application to achieve the predetermined invention purpose, the specific implementation methods, features and effects of the present application are described in detail below in combination with the preferred embodiments. Embodiment 1
[0032] This embodiment provides a preparation process of nano-silicon dioxide microcapsules, which is as follows:
[0033] Step 1: 30 g of polyethylene glycol octylphenyl ether, 12 g of isocyanatepropyltriethoxysilane and 8 g of dibutyltin dilaurate were mixed, heated in a water bath, and when the solution temperature was 50° C., the temperature was maintained constant, stirred for 20 h at a speed of 120 r / min, and a mixed reaction system 1 was obtained by reaction;
[0034] Step 2: Add 10 g of nano-silicon dioxide to the mixed reaction system 1, adjust the pH value to 8 with ammonia water, heat to 60° C. and stir for 24 h at a speed of 120 r / min to obtain a mixed reaction system 2;
[0035] Step 3: nitrogen is introduced into the mixed reaction system 2 for nitrogen deoxygenation at a nitrogen flow rate of 12 m / s. The temperature is raised to 70°C and stirred for 24 h at a rotation speed of 120 r / min to obtain a mixed reaction system 3. The solid-liquid separation is performed by suction filtration. The obtained solid is vacuum dried at 50°C for 12 h to obtain nano-silica microcapsules. Embodiment 2
[0036] This embodiment provides a preparation process of nano-silicon dioxide microcapsules, which is as follows:
[0037] Step 1: 40 g of polyethylene glycol octylphenyl ether, 10 g of isocyanatepropyltriethoxysilane and 10 g of dibutyltin dilaurate were mixed, and heated in a water bath. When the solution temperature was 40° C., the temperature was maintained constant, and the mixture was stirred for 24 h at a speed of 120 r / min to obtain a mixed reaction system 1.
[0038] Step 2: Add 10 g of nano-silicon dioxide to the mixed reaction system 1, adjust the pH value to 7 with ammonia water, heat to 75° C. and stir for 20 h at a speed of 120 r / min to obtain a mixed reaction system 2;
[0039] Step 3: nitrogen is introduced into the mixed reaction system 2 for nitrogen deoxygenation at a nitrogen flow rate of 12 m / s. The temperature is raised to 60°C and stirred for 28 hours at a rotation speed of 120 r / min to obtain a mixed reaction system 3. The solid-liquid separation is performed by suction filtration. The obtained solid is vacuum dried at 50°C for 12 hours to obtain nano-silica microcapsules. Embodiment 3
[0040] This embodiment provides a preparation process of nano-silicon dioxide microcapsules, which is as follows:
[0041] Step 1: 50 g of polyethylene glycol octylphenyl ether, 8 g of isocyanatepropyltriethoxysilane and 12 g of dibutyltin dilaurate were mixed, and heated in a water bath. When the solution temperature was 60° C., the temperature was maintained constant, and the mixture was stirred for 16 h at a speed of 120 r / min to obtain a mixed reaction system 1.
[0042] Step 2: Add 10 g of nano-silicon dioxide to the mixed reaction system 1, adjust the pH value to 9 with aqueous ammonia, heat to 55° C. and stir for 28 h at a speed of 120 r / min to obtain a mixed reaction system 2;
[0043] Step 3: nitrogen is introduced into the mixed reaction system 2 for nitrogen deoxygenation at a nitrogen flow rate of 12 m / s. The temperature is raised to 80°C and stirred for 20 h at a rotation speed of 120 r / min to obtain a mixed reaction system 3. The solid-liquid separation is performed by suction filtration. The obtained solid is vacuum dried at 50°C for 12 h to obtain nano-silica microcapsules. Embodiment 4
[0044] This embodiment provides a method for preparing a self-cleaning agricultural anti-fog shed film, which is as follows:
[0045] Step S1. Methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate are mixed in a mass ratio of 60:70:15):1:150, nitrogen is introduced, the flow rate of nitrogen is 12 m / s, the reaction temperature is 75°C, the stirring time is 11 h, the speed is 150 r / min, and the mixture is stirred to obtain a mixed solution A;
[0046] Step S2. Methanol was added to the mixed solution A, the mass ratio of methanol to the mixed solution A being 1:70, the obtained precipitate was washed with ethyl alcohol, and vacuum dried at 50° C. for 13 h to obtain a solid sample;
[0047] Step S3. Add 1% nano-silicon dioxide suspension by mass to the solid sample obtained in step S2, and mix them, control the mass ratio of the solid sample to the nano-silicon dioxide suspension to be 1:75, ultrasonically treat at room temperature for 25 minutes, and then stir for 40 minutes to obtain a mixed solution B for standby use;
[0048] Step S4. The silane coupling agent, high-density polyethylene, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and nano-silica microcapsules are mixed in a mass ratio of 85:4:2:3, the temperature of the feeding section is controlled to be 80°C, the temperature of the melt mixing section is controlled to be 110°C, the temperature of the metering section is controlled to be 160°C, the temperature of the die head is controlled to be 170°C, and the plastic film is obtained by blowing;
[0049] Step S5. Spin-coat the mixed solution B obtained in step S3 onto the surface of the plastic film in step S4 at a spin-coating speed of 2000 r / min for 20 s, and dry with air at 40° C. to obtain a self-cleaning agricultural anti-fog shed film. Embodiment 5
[0050] This embodiment provides a method for preparing a self-cleaning agricultural anti-fog shed film, which is as follows:
[0051] Step S1. Methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate are mixed in a mass ratio of 70:60:20:1:160, nitrogen is introduced, the flow rate of nitrogen is 12 m / s, the reaction temperature is 80° C., the stirring time is 12 h, the rotation speed is 150 r / min, and the mixture is stirred to obtain a mixed solution A;
[0052] Step S2. Methanol was added to the mixed solution A, the mass ratio of methanol to the mixed solution A being 1:80, the obtained precipitate was washed with ethyl alcohol, and vacuum dried at 40° C. for 12 h to obtain a solid sample;
[0053] Step S3. Add 1% nano-silica suspension by mass fraction to the solid sample obtained in step S2 for mixing, control the mass ratio of the solid sample to the nano-silica suspension to be 1:100, ultrasonically treat at room temperature for 30 minutes, and then stir for 30 minutes to obtain a mixed solution B for standby use;
[0054] Step S4. The silane coupling agent, high-density polyethylene, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and nano-silica microcapsules are mixed in a mass ratio of 80:5:3:2, the feeding section temperature is controlled to be 100° C., the melt mixing section temperature is controlled to be 120° C., the metering section temperature is controlled to be 150° C., the die head temperature is controlled to be 180° C., and the plastic film is obtained by blowing;
[0055] Step S5. Spin-coat the mixed solution B obtained in step S3 onto the surface of the plastic film in step S4 at a spin-coating speed of 2000 r / min for 20 s, and dry with air at 40° C. to obtain a self-cleaning agricultural anti-fog shed film. Embodiment 6
[0056] This embodiment provides a method for preparing a self-cleaning agricultural anti-fog shed film, which is as follows:
[0057] Step S1. Methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate are mixed in a mass ratio of 50:80:10:1:140, nitrogen is introduced, the flow rate of nitrogen is 12 m / s, the reaction temperature is 70° C., the stirring time is 10 h, the rotation speed is 150 r / min, and the mixture is stirred to obtain a mixed solution A;
[0058] Step S2. Methanol was added to the mixed solution A, the mass ratio of methanol to the mixed solution A being 1:60, the obtained precipitate was washed with ethyl alcohol, and vacuum dried at 60° C. for 15 h to obtain a solid sample;
[0059] Step S3. Add 1% nano-silica suspension by mass fraction to the solid sample obtained in step S2, and mix them, control the mass ratio of the solid sample to the nano-silica suspension to be 1:50, ultrasonically treat at room temperature for 20 minutes, and then stir for 60 minutes to obtain a mixed solution B for standby use;
[0060] Step S4. The silane coupling agent, high-density polyethylene, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and nano-silica microcapsules are mixed in a mass ratio of 90:3:1:4, the feeding section temperature is controlled to be 60°C, the melt mixing section temperature is 100°C, the metering section temperature is 170°C, the die head temperature is 150°C, and the plastic film is inflated;
[0061] Step S5. Spin-coat the mixed solution B obtained in step S3 onto the surface of the plastic film in step S4 at a spin-coating speed of 2000 r / min for 20 s, and dry with air at 40° C. to obtain a self-cleaning agricultural anti-fog shed film. Embodiment 7
[0062] This embodiment provides a method for preparing a self-cleaning agricultural anti-fog shed film, which is as follows:
[0063] Step S1. Methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate are mixed in a mass ratio of 65:80:17:1:153, nitrogen is introduced, the flow rate of nitrogen is 12 m / s, the reaction temperature is 70° C., the stirring time is 11 h, the rotation speed is 150 r / min, and the mixture is stirred to obtain a mixed solution A;
[0064] Step S2. Methanol was added to the mixed solution A, the mass ratio of methanol to the mixed solution A being 1:78, the obtained precipitate was washed with ethyl alcohol, and vacuum dried at 55° C. for 14 h to obtain a solid sample;
[0065] Step S3. Add 1% nano-silica suspension by mass to the solid sample obtained in step S2, and mix them, control the mass ratio of the solid sample to the nano-silica suspension to be 1:90, ultrasonically treat at room temperature for 22 minutes, and then stir for 55 minutes to obtain a mixed solution B for standby use;
[0066] Step S4. The silane coupling agent, high-density polyethylene, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and nano-silica microcapsules are mixed in a mass ratio of 88:4:2:4, the feeding section temperature is controlled to be 85°C, the melt mixing section temperature is controlled to be 110°C, the metering section temperature is controlled to be 165°C, the die head temperature is controlled to be 160°C, and the plastic film is obtained by blowing;
[0067] Step S5. Spin-coat the mixed solution B obtained in step S3 onto the surface of the plastic film in step S4 at a spin-coating speed of 2000 r / min for 20 s, and dry with air at 40° C. to obtain a self-cleaning agricultural anti-fog shed film.
[0068] Comparative Example 1
[0069] The main difference between this comparative example and Example 4 is that no nano-silicon dioxide microcapsules are added in this comparative example.
[0070] Comparative Example 2
[0071] The main difference between this comparative example and Example 4 is that in this comparative example, no nano-silicon dioxide suspension is added in step S3.
[0072] Performance Testing
[0073] The anti-fog performance of the greenhouse film prepared in this application was tested with reference to GB / T 31726-2015 "Test method for anti-fog performance of plastic films"; and the contact angle of the product was tested (the contact angle can measure the hydrophobicity of the product. If θ<90°, the solid surface is hydrophilic, that is, the liquid is easier to wet the solid, and the smaller the angle, the better the wettability; if θ>90°, the solid surface is hydrophobic, that is, the liquid is not easy to wet the solid and is easy to move on the surface). The results are shown in Table 1.
[0074] Table 1
[0075] sample Anti-fog level Contact angle θ (initial) Contact angle θ (after 5 months of use) Example 4 Level I 135° 132° Example 5 Level I 128° 126° Example 6 Level I 131° 129° Example 7 Level I 126° 124° Comparative Example 1 Level I 127° 102° Comparative Example 2 Level II 115° 98° Comparative samples Level II 120° 65°
[0076] Note: The comparison samples in the table are similar products purchased from the same category and are only used for comparison tests.
[0077] Result analysis:
[0078] It can be seen from Table 1 that the samples prepared in the present application have good anti-fog performance and hydrophobicity, and can achieve a good self-cleaning effect. After five months of use, the contact angle was tested by sampling. The contact angle of the greenhouse film prepared by the process of the present application decreased slightly and almost remained stable, thus prolonging the anti-fog and self-cleaning effect of the greenhouse film. However, the effect of the comparative example and comparative samples decreased significantly after 5 months of use. It may be that the hydrophobic coating was damaged during long-term use and could not heal itself.
[0079] The above is only a preferred embodiment of the present application and does not constitute any form of limitation to the present application. Although the present application has been disclosed as a preferred embodiment as above, it is not intended to limit the present application. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present application. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application are still within the scope of the technical solution of the present application.
Claims
1. A method for preparing a self-cleaning agricultural anti-fog shed film, It is characterized in that The steps include: Step S1. Methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate are mixed and stirred to obtain a mixed solution A, wherein the mass ratio of methyl methacrylate, polydimethylsiloxane, silane coupling agent, azobisisobutyronitrile and ethyl acetate is (50-70):(60-80):(10-20):1:(140-160); Step S2. Methanol is added to the mixed solution A, the obtained precipitate is washed with a detergent, and vacuum dried to obtain a solid sample; Step S3. Add the nano-silicon dioxide suspension to the solid sample obtained in step S2 and mix them to obtain a mixed solution B for standby use; Step S4. Mixing and inflating a silane coupling agent, high-density polyethylene, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and nano-silica microcapsules to obtain a plastic film, wherein the mass ratio of the high-density polyethylene, the silane coupling agent, pentaerythritol tetra(bis-T-butyl hydroxyhydrocinnamate) ester and the nano-silica microcapsules is (80-90): (3-5): (1-3): (2-4); The preparation method of the nano silicon dioxide microcapsule is as follows: Step S41. reacting polyethylene glycol octylphenyl ether, isocyanate propyltriethoxysilane and dibutyltin dilaurate to obtain a mixed reaction system 1; Step S42. Add nano-silicon dioxide to the mixed reaction system 1, adjust the pH value to 7-9, and react to obtain a mixed reaction system 2; Step S43. Deoxygenating the mixed reaction system 2 with nitrogen, continuing the reaction to obtain a mixed reaction system 3, followed by solid-liquid separation, and drying the obtained solid to obtain nano-silicon dioxide microcapsules; The mass ratio of polyethylene glycol octylphenyl ether, isocyanate propyl triethoxysilane, dibutyltin dilaurate and nano-silicon dioxide is (3-5): (0.8-1.2): (0.8-1.2): 1; the reaction conditions of step S41 are stirring at 40-60°C for 16-24 hours; the reaction conditions of step S42 are stirring at 55-75°C for 20-28 hours, and the reaction conditions of step S43 are stirring at 60-80°C for 20-28 hours; Step S5. Spin-coat the mixed solution B obtained in step S3 onto the surface of step S4 to obtain a self-cleaning agricultural anti-fog shed film.
2. A method for preparing a self-cleaning agricultural anti-fog shed film according to claim 1, It is characterized in that The reaction temperature in step S1 is 70-80° C., the stirring time is 10-12 h, and the stirring reaction needs to be completed in a nitrogen atmosphere.
3. A method for preparing a self-cleaning agricultural anti-fog shed film according to claim 1, It is characterized in that In step S2, the mass ratio of methanol to mixed liquid A is 1: (60-80), the detergent is ethyl alcohol, the washing times are 2-3 times, the vacuum drying temperature is 40-60° C., and the vacuum drying time is 12-15 hours.
4. A method for preparing a self-cleaning agricultural anti-fog shed film according to claim 1, It is characterized in that In step S3, the mass fraction of the nano-silicon dioxide suspension is 1%, the mass ratio of the solid sample to the nano-silicon dioxide suspension is 1:(50-100), and the mixing treatment is ultrasonic treatment at room temperature for 20-30 minutes, followed by stirring for 30-60 minutes.
5. A method for preparing a self-cleaning agricultural anti-fog shed film according to claim 1, It is characterized in that The inflation in step S4 adopts multi-stage temperature control, wherein the temperature of the feeding section is controlled at 60-100°C, the temperature of the melt mixing section is controlled at 100-120°C, the temperature of the metering section is controlled at 150-170°C, and the temperature of the die head is controlled at 150-180°C.