A flame-retardant cable with high insulation and its production process

By using microcapsule flame retardant additives, modified magnesium hydroxide and silane coupling agents in cable insulation materials to form a microcapsule structure and coated with an organic protective layer, the problem of cables being prone to fire and water absorption leading to a decrease in insulation performance is solved and improved Improved flame retardant effect and insulation performance.

CN118290868BActive Publication Date: 2024-10-01GUANGDONG ZHONGDE CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410365110.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-27
Publication Date
2024-10-01
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

Existing cable insulation materials are easy to catch fire, produce toxic gases and smoke when burning, and the insulation performance decreases during the water absorption process. The flame retardant has poor compatibility with the base material, which limits its application.

Method used

Microcapsule flame retardant additives are added to the polyvinyl chloride matrix, and a microcapsule structure is formed by modifying magnesium hydroxide and silane coupling agent to reduce water absorption, and the surface is coated with an organic protective layer containing a phosphorus structure to inhibit combustion.

Benefits of technology

It improves the flame retardant effect and insulation performance of the cable, especially under wet conditions, delays the burning speed, enhances the flame retardant performance and mechanical strength, and solves the problem of low efficiency of single-component flame retardants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004763988340000021
    Figure BDA0004763988340000021
  • Figure BDA0004763988340000031
    Figure BDA0004763988340000031
  • Figure BDA0004763988340000032
    Figure BDA0004763988340000032
Patent Text Reader

Abstract

The invention relates to a flame-retardant cable with high insulation and a production process thereof, belonging to the technical field of cables. The cable comprises a cable core and an insulating flame-retardant protective layer on the surface thereof, wherein the insulating flame-retardant protective layer comprises, by weight, 100 parts of polyvinyl chloride, 20-30 parts of a plasticizer, 10-20 parts of a microcapsule flame-retardant additive, 0.5-0.8 parts of a lubricant, 2-3 parts of a stabilizer, 1-1.5 parts of an antioxidant and 1-1.5 parts of a pigment; wherein the microcapsule flame-retardant additive can not only alleviate the phenomenon that the insulation performance of the polyvinyl chloride body is reduced due to water absorption and soaking of magnesium hydroxide during use, but also can decompose a phosphorus-containing structure at the early stage of a fire to inhibit a free radical chain reaction and absorb heat from a combustion zone, thereby further delaying the combustion speed; when the fire continues to occur, the magnesium hydroxide in the microcapsule flame-retardant additive can be released, thereby generating a synergistic effect and reinforcing the flame-retardant performance of the insulating flame-retardant protective layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cables, and specifically relates to a high-insulation flame-retardant cable and a production process thereof. Background Art

[0002] In power lines, the proportion of cables is gradually increasing. Power cables are cable products used to transmit and distribute high-power electric energy in the trunk lines of power systems, including power cables of various voltage levels and insulation levels of 1-500KV and above.

[0003] Cable insulation materials are generally required to have excellent long-term aging resistance, radiation resistance, stable electrical properties, flame retardancy and insulation properties. Currently, commonly used cable insulation materials are polyethylene, polyvinyl chloride, ethylene propylene rubber and other materials, but the main disadvantage of these base materials is that they are easy to ignite and cause fires. Halogen-containing flame retardant materials, such as flame retardant polyvinyl chloride, have better flame retardant effects, but when burned, they will produce toxic hydrogen chloride gas and a lot of smoke, causing poisoning and suffocation, hindering the evacuation of personnel and the progress of fire fighting, causing loss of life and property. Current insulation materials usually use inorganic flame retardants, such as aluminum hydroxide, magnesium hydroxide, etc. The added inorganic flame retardants themselves are not flame retardant, but when opened at 350°C, they will ignite and cause fires. Decomposition begins to occur, and the metal oxides produced by the decomposition adhere to the surface of the organic matter, which can prevent the organic matter from further burning. The decomposition itself needs to absorb a large amount of heat, which reduces the combustion temperature. In addition, the water vapor produced by the decomposition can absorb a certain amount of smoke, which has a good flame retardant effect. However, since the added inorganic flame retardant itself has a high water absorption capacity, it is easy to absorb moisture during use, and water itself is a conductive medium, so the insulation performance of the existing cable insulation material is reduced during the wetting process. In addition, the current inorganic flame retardant is not compatible with the organic base material and is easy to migrate to the plastic surface, resulting in a decrease in its insulation and flame retardant properties, further limiting its application in the cable field. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a flame-retardant cable with high insulation and a production process thereof;

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-insulation flame-retardant cable comprises a cable core and an insulating flame-retardant protective layer on the surface thereof; the insulating flame-retardant protective layer comprises the following raw materials in parts by weight:

[0007] 100 parts of polyvinyl chloride, 20-30 parts of plasticizer, 10-20 parts of microcapsule flame retardant additive, 0.5-0.8 parts of lubricant, 2-3 parts of stabilizer, 1-1.5 parts of antioxidant and 1-1.5 parts of pigment;

[0008] Preparation of microcapsule flame retardant additives:

[0009] Step A1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride are mixed and added into a reaction kettle, the temperature is raised to 60-70° C., pentaerythritol triallyl ether is added dropwise into the reaction kettle at 200-300 r / min, the mixture is refluxed and reacted at a constant temperature for 2-3 hours, a 25% by mass sodium hydroxide solution is added into the mixed solution, the temperature is raised to 75° C., the reaction is continued with stirring for 3 hours, and the intermediate 1 is obtained by rotary evaporation under reduced pressure;

[0010] Further, the amount ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride is 0.15 mol: 0.1 mol: 0.5-0.8 g: 15 mL: 50 mL;

[0011] Epichlorohydrin is ring-opened under the catalysis of boron trifluoride ether to form chlorohydrin, and then HCl is removed under alkaline conditions and the ring is closed to introduce epoxy groups. Its structural formula is as follows:

[0012]

[0013] Step A2: DOPO, triphenylphosphine and DMF are mixed and added to a reactor, the temperature is raised to 110-120°C, and intermediate 1 is added dropwise to the reactor at 150-200 r / min. After the reaction is stirred for 1-2 hours, the reaction is washed with water 2-3 times to remove DMF, and then the reaction is transferred to an oven and dried for 5 hours to obtain intermediate 2;

[0014] Further, the usage ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.3-0.5 g: 80 mL;

[0015] The PH in DOPO can undergo addition reaction with epoxy groups and be replaced by PC to form DOPO derivatives, the structure of which is as follows:

[0016]

[0017] Step A3: diethylenetriamine, sodium ethoxide and toluene are mixed and added into a reaction kettle, the temperature is raised to 30-40°C, intermediate 2 is added dropwise into the reaction kettle at 200-300r / min, the reaction is stirred and kept warm for 3-4h, and then vacuum rotary evaporation is performed to obtain intermediate 3;

[0018] Further, the usage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene is 0.15 mol: 0.05 mol: 10-15 mL: 100 mL;

[0019] The secondary amine structure in diethylenetriamine and the double bond in intermediate 2 undergo Michael addition reaction to form an amino-terminated multi-branched intermediate; its structure is as follows:

[0020]

[0021] Step A4: intermediate 3, triethylamine and THF are mixed and added into a reaction kettle, p-toluenesulfonyl chloride is added dropwise into the reaction kettle at 300-500 r / min, and sodium hydroxide and propylene chloride are added dropwise after stirring at room temperature for 8-10 hours, and the temperature is raised to 40-50°C, and the reaction is stirred at this temperature for 1-2 hours, and then the intermediate 4 is obtained by rotary evaporation under reduced pressure;

[0022] Further, the usage ratio of intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2-2.5 g: 0.12 mol: 0.02 mol: 1-1.5 g: 150 mL;

[0023] p-Toluenesulfonyl chloride is used to protect the amino group on intermediate 3 under the catalytic action of triethylamine, and then the alcoholic hydroxyl group on intermediate 3 reacts with allyl chloride to introduce an unsaturated double bond on intermediate 3;

[0024] Step A5: Put magnesium hydroxide and ethanol solution in a beaker, control the stirring reaction rate to 500-800r / min, stir for 20min, then add A174, heat to 25-30°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide;

[0025] Furthermore, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.5-0.8g:200mL; the mass fraction of ethanol solution is 60%;

[0026] Magnesium hydroxide is modified by a wet process, and a silane coupling agent is grafted onto the magnesium hydroxide, thereby reducing the water absorption of the magnesium hydroxide and introducing an unsaturated double bond structure;

[0027] Step A6: taking intermediate 4, modified magnesium hydroxide, AIBN initiator and THF, mixing and feeding them into a reactor, controlling the stirring reaction rate to be 200-300 r / min, heating to 50-60°C, stirring and reacting for 4-5 hours under reduced pressure, and then rotary evaporating to obtain a crude microcapsule flame retardant additive, and then mixing the crude product, hydrogen bromide acetic acid solution and phenol into a reactor, controlling the stirring reaction rate to be 200-300 r / min, heating to 60-70°C, stirring and reacting for 1 hour under heated condition, washing with anhydrous ethanol 2-3 times, and transferring to an oven for drying to obtain a microcapsule flame retardant additive;

[0028] Further, the usage ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, hydrogen bromide acetic acid solution, phenol and THF is 10 g: 3-5 g: 0.2-0.3 g: 50 mL: 11.5 g: 200 mL;

[0029] The unsaturated double bonds on the intermediate 4 and the unsaturated double bonds on the modified magnesium hydroxide are copolymerized under the action of the AIBN initiator to form a low molecular weight copolymer to coat the modified magnesium hydroxide to form microcapsules, and then the benzenesulfonyl group in the low molecular weight copolymer is removed with a mixture of hydrogen bromide acetic acid solution and phenol, and the amino group on the low molecular weight polymer is deprotected to obtain a microcapsule flame retardant additive containing amino groups on the surface.

[0030] Preparation of flame-retardant cables with high insulation:

[0031] Step S1: mixing a microcapsule flame retardant additive, a lubricant, a stabilizer, an antioxidant and a pigment into a stirrer to prepare a functional mixture;

[0032] Step S2: Mix polyvinyl chloride resin, plasticizer and functional mixture and feed them into a twin-screw extruder, adjust the temperature of each zone of the twin-screw to 140-150°C, 150-170°C, 170-190°C, 200-220°C, 200-220°C, 190-200°C, apply 70-80r / min, and the extrusion mass flow rate is 30-40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0033] Beneficial effects of the present invention:

[0034] The invention discloses a high-insulation flame-retardant cable, comprising a cable core and an insulating flame-retardant protective layer on the surface, wherein the insulating flame-retardant protective layer is prepared by adding a microcapsule flame-retardant additive to a polyvinyl chloride substrate. Compared with the existing polyvinyl chloride substrate, the introduction of the microcapsule flame-retardant additive improves the flame-retardant effect of the insulating flame-retardant protective layer while still achieving good insulating performance under soaking conditions.

[0035] The magnesium hydroxide is grafted and modified by a silane coupling agent and copolymerized, and an organic protective layer is coated on its surface to form a microcapsule structure. On the one hand, the magnesium hydroxide can be isolated from the external environment, reducing its hydrophilicity and water absorption, and effectively alleviating the phenomenon that the insulation performance of the polyvinyl chloride body is reduced due to water absorption and soaking of the magnesium hydroxide during use; on the other hand, the phosphorus-containing structure on the organic protective layer has a low decomposition temperature. In the early stage of a fire, the phosphorus-containing structure will first be thermally decomposed to produce phosphorus free radicals to capture active intermediates of the combustion reaction, inhibit the free radical chain reaction, and reduce its combustion rate. The thermal decomposition will absorb the heat of the combustion zone, reduce the temperature of the combustion zone, and even drop to below the critical point of the combustion temperature, further delaying its combustion rate; when the fire continues to occur and the temperature of the combustion zone continues to rise, the magnesium hydroxide in the microcapsule flame retardant additive will be released, and the metal oxides produced by the decomposition will adhere to the surface of the organic matter, which can further prevent the combustion of the organic matter. The phosphorus-containing structure of the organic protective layer and the magnesium hydroxide in the microcapsule structure produce a synergistic effect, effectively solving the defect of low efficiency of the single-component flame retardant, and further strengthening the flame retardant performance of the insulating flame retardant protective layer.

[0036] Moreover, the multi-branched structure of the terminal amino group on the microcapsule flame retardant additive can cross-link with the chlorine element on the polyvinyl chloride, which can reduce the migration of the microcapsule flame retardant additive in the polyvinyl chloride matrix, and can also "stick" multiple polyvinyl chloride molecular chains together to improve its mechanical strength. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] The raw materials for preparing the flame-retardant cables with high insulation properties in the embodiments and comparative examples are shown in Table 1:

[0039] Table 1

[0040]

[0041] Example 1

[0042] The specific implementation process of preparing a high-insulation flame-retardant cable in this embodiment is as follows:

[0043] 1) Preparation of microcapsule flame retardant additives

[0044] a1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride were mixed and added into a reactor, and the temperature was raised to 60°C. Pentaerythritol triallyl ether was added dropwise into the reactor at 200 r / min, and the mixture was refluxed and reacted at a constant temperature for 2 hours. Then, a 25% sodium hydroxide solution was added into the mixed solution, and the temperature was raised to 75°C. After stirring and reacting for 3 hours, the intermediate 1 was obtained by rotary evaporation under reduced pressure. In the above reaction, the dosage ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride was 0.15 mol: 0.1 mol: 0.5 g: 15 mL: 50 mL.

[0045] a2: DOPO, triphenylphosphine and DMF were mixed and added to a reactor, and the temperature was raised to 110°C. Intermediate 1 was added dropwise to the reactor at 150 r / min. After stirring and reacting for 1 hour, the mixture was washed with water twice to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2. In the above reaction, the ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.3 g: 80 mL.

[0046] a3: Diethylenetriamine, sodium ethoxide and toluene are mixed and added into a reactor, and the temperature is raised to 30°C. At 200 r / min, intermediate 2 is added dropwise into the reactor, and the mixture is stirred and reacted for 3 hours under reduced pressure and then rotary evaporated to obtain intermediate 3. In the above reaction, the dosage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene is 0.15 mol: 0.05 mol: 10 mL: 100 mL.

[0047] a4: Mix the intermediate 3, triethylamine and THF and feed them into a reactor. At 300 r / min, add p-toluenesulfonyl chloride dropwise into the reactor. Stir at room temperature for 8 h, then continue to add sodium hydroxide and allyl chloride dropwise. Heat to 40°C, stir and react for 1 h, then evaporate under reduced pressure to obtain the intermediate 4. In the above reaction, the ratio of the intermediate 3, triethylamine, p-toluenesulfonyl chloride, allyl chloride, sodium hydroxide and THF is 0.02 mol: 2 g: 0.12 mol: 0.02 mol: 1 g: 150 mL.

[0048] a5: Put magnesium hydroxide and 60% ethanol solution in a beaker, control the stirring reaction rate to 500r / min, stir for 20min, then add A174, heat to 25°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide; in the above reaction, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.5g:200mL;

[0049] a6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF and mix them into a reactor, control the stirring reaction rate to 200r / min, heat to 50°C, keep stirring and react for 4h, and then vacuum evaporation to obtain a crude microcapsule flame retardant additive. Then, mix the crude product, hydrogen bromide acetic acid solution and phenol and feed them into a reactor, control the stirring reaction rate to 200r / min, heat to 60°C, keep stirring and react for 1h, wash twice with anhydrous ethanol, and transfer to an oven to dry to obtain a microcapsule flame retardant additive; in the above reaction, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, trifluoroacetic acid and THF is 10g:3g:0.2g:50mL:11.5g:200mL;

[0050] 2) Preparation of flame-retardant cables with high insulation

[0051] s1: 10 parts of microcapsule flame retardant additive, 0.5 parts of lubricant, 2 parts of stabilizer, 1 part of antioxidant and 1 part of pigment are mixed and added into a blender to prepare a functional mixture;

[0052] s2: Mix 100 parts of polyvinyl chloride resin, 20 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 140℃, 150℃, 170℃, 200℃, 200℃ and 190℃, apply 70r / min, and the extrusion mass flow rate is 30kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0053] Example 2

[0054] The specific implementation process of preparing a high-insulation flame-retardant cable in this embodiment is as follows:

[0055] 1) Preparation of microcapsule flame retardant additives

[0056] a1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride were mixed and added into a reactor, and the temperature was raised to 62°C. Pentaerythritol triallyl ether was added dropwise into the reactor at 220 r / min, and the mixture was refluxed and reacted at a constant temperature for 2 hours. Then, a 25% sodium hydroxide solution was added into the mixed solution, and the temperature was raised to 75°C. After stirring and reacting for 3 hours, the intermediate 1 was obtained by rotary evaporation under reduced pressure. In the above reaction, the dosage ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride was 0.15 mol: 0.1 mol: 0.6 g: 15 mL: 50 mL.

[0057] a2: DOPO, triphenylphosphine and DMF were mixed and added to a reactor, and the temperature was raised to 112°C. Intermediate 1 was added dropwise to the reactor at 200 r / min. After stirring and reacting for 1 hour, the mixture was washed with water for 3 times to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2. In the above reaction, the ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.4 g: 80 mL.

[0058] a3: Diethylenetriamine, sodium ethoxide and toluene are mixed and added into a reactor, and the temperature is raised to 32°C. At 250 r / min, intermediate 2 is added dropwise into the reactor, and the mixture is stirred and reacted for 4 hours under reduced pressure and then rotary evaporated to obtain intermediate 3. In the above reaction, the dosage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene is 0.15 mol: 0.05 mol: 11 mL: 100 mL.

[0059] a4: Mix the intermediate 3, triethylamine and THF and feed them into a reactor. At 350 r / min, add p-toluenesulfonyl chloride dropwise into the reactor. Stir at room temperature for 9 hours and then continue to add sodium hydroxide and propylene chloride dropwise. Heat to 42°C, stir and react for 2 hours under reduced pressure and rotary evaporate to obtain the intermediate 4. In the above reaction, the amount ratio of the intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2.1 g: 0.12 mol: 0.02 mol: 1.1 g: 150 mL.

[0060] a5: Put magnesium hydroxide and 60% ethanol solution in a beaker, control the stirring reaction rate to 600r / min, stir for 20min, then add A174, heat to 26°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide; in the above reaction, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.6g:200mL;

[0061] a6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF and mix them into a reactor, control the stirring reaction rate to 220r / min, heat to 52°C, keep stirring and react for 4h, then evaporate under reduced pressure to obtain a crude microcapsule flame retardant additive, then mix the crude product, hydrogen bromide acetic acid solution and phenol and mix them into a reactor, control the stirring reaction rate to 220r / min, heat to 62°C, keep stirring and react for 1h, wash with anhydrous ethanol 3 times, transfer to an oven and dry to obtain a microcapsule flame retardant additive; in the above reaction, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, trifluoroacetic acid and THF is 10g:3g:0.3g:50mL:11.5g:200mL;

[0062] 2) Preparation of flame-retardant cables with high insulation

[0063] s1: 12 parts of microcapsule flame retardant additive, 0.6 parts of lubricant, 3 parts of stabilizer, 1.1 parts of antioxidant and 1.1 parts of pigment are mixed and added into a blender to prepare a functional mixture;

[0064] s2: Mix 100 parts of polyvinyl chloride resin, 22 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 145℃, 160℃, 180℃, 210℃, 210℃ and 200℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0065] Example 3

[0066] The specific implementation process of preparing a high-insulation flame-retardant cable in this embodiment is as follows:

[0067] 1) Preparation of microcapsule flame retardant additives

[0068] a1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride were mixed and added into a reactor, and the temperature was raised to 64°C. Pentaerythritol triallyl ether was added dropwise into the reactor at 240 r / min, and the mixture was refluxed and reacted at a constant temperature for 2 hours. Then, a 25% sodium hydroxide solution was added into the mixed solution, and the temperature was raised to 75°C. After stirring and reacting for 3 hours, the intermediate 1 was obtained by rotary evaporation under reduced pressure. In the above reaction, the dosage ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride was 0.15 mol: 0.1 mol: 0.7 g: 15 mL: 50 mL.

[0069] a2: DOPO, triphenylphosphine and DMF were mixed and added to a reactor, and the temperature was raised to 114°C. Intermediate 1 was added dropwise to the reactor at 200 r / min. After stirring and reacting for 2 hours, the mixture was washed with water for 3 times to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2. In the above reaction, the ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.5 g: 80 mL.

[0070] a3: Diethylenetriamine, sodium ethoxide and toluene were mixed and added into a reactor, and the temperature was raised to 34°C. At 300 r / min, intermediate 2 was added dropwise into the reactor, and the mixture was stirred and reacted for 3 hours under reduced pressure and rotary evaporation was performed to obtain intermediate 3. In the above reaction, the dosage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene was 0.15 mol: 0.05 mol: 12 mL: 100 mL.

[0071] a4: Mix the intermediate 3, triethylamine and THF and feed them into a reactor. At 400 r / min, add p-toluenesulfonyl chloride dropwise into the reactor. Stir at room temperature for 9 hours and then continue to add sodium hydroxide and propylene chloride dropwise. Heat to 44°C, stir and react for 2 hours under reduced pressure and rotary evaporate to obtain the intermediate 4. In the above reaction, the amount ratio of the intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2.2 g: 0.12 mol: 0.02 mol: 1.2 g: 150 mL.

[0072] a5: Put magnesium hydroxide and 60% ethanol solution in a beaker, control the stirring reaction rate to 700r / min, stir for 20min, then add A174, heat to 27°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide; in the above reaction, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.7g:200mL;

[0073] a6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF and mix them into a reactor, control the stirring reaction rate to 240r / min, heat to 54°C, keep stirring and react for 4h, and then evaporate under reduced pressure to obtain a crude microcapsule flame retardant additive. Then, mix the crude product, hydrogen bromide acetic acid solution and phenol and mix them into a reactor, control the stirring reaction rate to 240r / min, heat to 64°C, keep stirring and react for 1h, wash with anhydrous ethanol for 3 times, and transfer to an oven to dry to obtain a microcapsule flame retardant additive; in the above reaction, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, trifluoroacetic acid and THF is 10g:3g:0.3g:50mL:11.5g:200mL;

[0074] 2) Preparation of flame-retardant cables with high insulation

[0075] s1: 14 parts of microcapsule flame retardant additive, 0.7 parts of lubricant, 3 parts of stabilizer, 1.2 parts of antioxidant and 1.2 parts of pigment are mixed and added into a blender to prepare a functional mixture;

[0076] s2: Mix 100 parts of polyvinyl chloride resin, 24 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 150℃, 170℃, 185℃, 215℃, 215℃ and 200℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0077] Example 4

[0078] The specific implementation process of preparing a high-insulation flame-retardant cable in this embodiment is as follows:

[0079] 1) Preparation of microcapsule flame retardant additives

[0080] a1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride were mixed and fed into a reactor, and the temperature was raised to 66°C. Pentaerythritol triallyl ether was added dropwise into the reactor at 260 r / min, and the mixture was refluxed and reacted at a constant temperature for 2 hours. Then, a 25% sodium hydroxide solution was added into the mixed solution, and the temperature was raised to 75°C. After stirring and reacting for 3 hours, the intermediate 1 was obtained by rotary evaporation under reduced pressure. In the above reaction, the dosage ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride was 0.15 mol: 0.1 mol: 0.8 g: 15 mL: 50 mL.

[0081] a2: DOPO, triphenylphosphine and DMF were mixed and added to a reactor, and the temperature was raised to 116°C. Intermediate 1 was added dropwise to the reactor at 200 r / min. After stirring and reacting for 2 hours, the mixture was washed with water for 3 times to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2. In the above reaction, the ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.5 g: 80 mL.

[0082] a3: Diethylenetriamine, sodium ethoxide and toluene were mixed and added into a reactor, and the temperature was raised to 36°C. At 300 r / min, intermediate 2 was added dropwise into the reactor, and the mixture was stirred and reacted for 3 hours under reduced pressure and then rotary evaporated to obtain intermediate 3. In the above reaction, the dosage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene was 0.15 mol: 0.05 mol: 13 mL: 100 mL.

[0083] a4: Mix the intermediate 3, triethylamine and THF and feed them into a reactor. At 450 r / min, add p-toluenesulfonyl chloride dropwise into the reactor. Stir at room temperature for 9 hours and then continue to add sodium hydroxide and propylene chloride dropwise. Heat to 46°C. Keep stirring and react for 2 hours and then evaporate under reduced pressure to obtain the intermediate 4. In the above reaction, the amount ratio of the intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2.3 g: 0.12 mol: 0.02 mol: 1.3 g: 150 mL.

[0084] a5: Put magnesium hydroxide and 60% ethanol solution in a beaker, control the stirring reaction rate to 800r / min, stir for 20min, then add A174, heat to 28°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide; in the above reaction, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.8g:200mL;

[0085] a6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF and mix them into a reactor, control the stirring reaction rate to 260r / min, heat to 56°C, keep stirring and react for 4h, then evaporate under reduced pressure to obtain a crude microcapsule flame retardant additive, then mix the crude product, hydrogen bromide acetic acid solution and phenol and feed them into a reactor, control the stirring reaction rate to 260r / min, heat to 66°C, keep stirring and react for 1h, wash with anhydrous ethanol 3 times, transfer to an oven and dry to obtain a microcapsule flame retardant additive; in the above reaction, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, trifluoroacetic acid and THF is 10g:3g:0.3g:50mL:11.5g:200mL;

[0086] 2) Preparation of flame-retardant cables with high insulation

[0087] s1: 16 parts of microcapsule flame retardant additive, 0.8 parts of lubricant, 3 parts of stabilizer, 1.3 parts of antioxidant and 1.3 parts of pigment are mixed and added into a blender to prepare a functional mixture;

[0088] s2: Mix 100 parts of polyvinyl chloride resin, 26 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 150℃, 170℃, 190℃, 220℃, 220℃ and 200℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0089] Example 5

[0090] The specific implementation process of preparing a high-insulation flame-retardant cable in this embodiment is as follows:

[0091] 1) Preparation of microcapsule flame retardant additives

[0092] a1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride were mixed and added into a reactor, and the temperature was raised to 68°C. Pentaerythritol triallyl ether was added dropwise into the reactor at 280 r / min, and the mixture was refluxed and reacted at a constant temperature for 2 hours. Then, a 25% sodium hydroxide solution was added into the mixed solution, and the temperature was raised to 75°C. After stirring and reacting for 3 hours, the intermediate 1 was obtained by rotary evaporation under reduced pressure. In the above reaction, the dosage ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride was 0.15 mol: 0.1 mol: 0.8 g: 15 mL: 50 mL.

[0093] a2: DOPO, triphenylphosphine and DMF were mixed and added to a reactor, and the temperature was raised to 118°C. Intermediate 1 was added dropwise to the reactor at 200 r / min. After stirring and reacting for 2 hours, the mixture was washed with water for 3 times to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2. In the above reaction, the ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.5 g: 80 mL.

[0094] a3: Diethylenetriamine, sodium ethoxide and toluene were mixed and added into a reactor, and the temperature was raised to 38°C. At 300 r / min, intermediate 2 was added dropwise into the reactor, and the mixture was stirred and reacted for 3 hours under reduced pressure and rotary evaporated to obtain intermediate 3. In the above reaction, the dosage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene was 0.15 mol: 0.05 mol: 14 mL: 100 mL.

[0095] a4: Mix the intermediate 3, triethylamine and THF and feed them into a reactor. At 450 r / min, add p-toluenesulfonyl chloride dropwise into the reactor. Stir at room temperature for 9 hours and then continue to add sodium hydroxide and propylene chloride dropwise. Heat to 46°C, stir and react for 2 hours under reduced pressure and rotary evaporate to obtain the intermediate 4. In the above reaction, the amount ratio of the intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2.4 g: 0.12 mol: 0.02 mol: 1.4 g: 150 mL.

[0096] a5: Put magnesium hydroxide and 60% ethanol solution in a beaker, control the stirring reaction rate to 800r / min, stir for 20min, then add A174, heat to 29°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide; in the above reaction, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.8g:200mL;

[0097] a6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF and mix them into a reactor, control the stirring reaction rate to 280r / min, heat to 58°C, keep stirring and react for 4h, and then evaporate under reduced pressure to obtain a crude microcapsule flame retardant additive. Then, mix the crude product, hydrogen bromide acetic acid solution and phenol and mix them into a reactor, control the stirring reaction rate to 280r / min, heat to 68°C, keep stirring and react for 1h, wash with anhydrous ethanol 3 times, and transfer to an oven to dry to obtain a microcapsule flame retardant additive; in the above reaction, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, trifluoroacetic acid and THF is 10g:3g:0.3g:50mL:11.5g:200mL;

[0098] 2) Preparation of flame-retardant cables with high insulation

[0099] s1: 18 parts of microcapsule flame retardant additive, 0.8 parts of lubricant, 3 parts of stabilizer, 1.4 parts of antioxidant and 1.4 parts of pigment are mixed and added into a blender to prepare a functional mixture;

[0100] s2: Mix 100 parts of polyvinyl chloride resin, 28 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 150℃, 170℃, 190℃, 220℃, 220℃ and 200℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0101] Example 6

[0102] The specific implementation process of preparing a high-insulation flame-retardant cable in this embodiment is as follows:

[0103] 1) Preparation of microcapsule flame retardant additives

[0104] a1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride were mixed and added into a reactor, and the temperature was raised to 70°C. Pentaerythritol triallyl ether was added dropwise into the reactor at 300 r / min, and the mixture was refluxed and reacted at constant temperature for 2 hours. Then, a 25% sodium hydroxide solution was added into the mixed solution, and the temperature was raised to 75°C. After stirring and reacting for 3 hours, the intermediate 1 was obtained by rotary evaporation under reduced pressure. In the above reaction, the dosage ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride was 0.15 mol: 0.1 mol: 0.8 g: 15 mL: 50 mL.

[0105] a2: DOPO, triphenylphosphine and DMF were mixed and added to a reactor, and the temperature was raised to 120°C. Intermediate 1 was added dropwise to the reactor at 200 r / min. After stirring and reacting for 2 hours, the mixture was washed with water for 3 times to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2. In the above reaction, the dosage ratio of DOPO, intermediate 1, triphenylphosphine and DMF was 0.1 mol: 0.1 mol: 0.5 g: 80 mL.

[0106] a3: Diethylenetriamine, sodium ethoxide and toluene are mixed and added into a reactor, and the temperature is raised to 40°C. At 300 r / min, intermediate 2 is added dropwise into the reactor, and the mixture is stirred and reacted for 4 hours under reduced pressure and rotary evaporated to obtain intermediate 3. In the above reaction, the dosage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene is 0.15 mol: 0.05 mol: 14 mL: 100 mL.

[0107] a4: Mix the intermediate 3, triethylamine and THF and feed them into a reactor. At 450 r / min, add p-toluenesulfonyl chloride dropwise into the reactor. Stir at room temperature for 9 hours and then continue to add sodium hydroxide and propylene chloride dropwise. Heat to 46°C, stir and react for 2 hours under reduced pressure and rotary evaporate to obtain the intermediate 4. In the above reaction, the amount ratio of the intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2.4 g: 0.12 mol: 0.02 mol: 1.4 g: 150 mL.

[0108] a5: Put magnesium hydroxide and 60% ethanol solution in a beaker, control the stirring reaction rate to 800r / min, stir for 20min, then add A174, heat to 29°C, stir for 2h, filter and wash, then transfer the filter cake to an oven and dry for 24h to obtain modified magnesium hydroxide; in the above reaction, the dosage ratio of magnesium hydroxide, A174 and ethanol solution is 50g:0.8g:200mL;

[0109] a6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF and mix them into a reactor, control the stirring reaction rate to 280r / min, heat to 58°C, keep stirring and react for 4h, and then vacuum evaporation to obtain a crude microcapsule flame retardant additive. Then, mix the crude product, hydrogen bromide acetic acid solution and phenol and feed them into a reactor, control the stirring reaction rate to 300r / min, heat to 70°C, keep stirring and react for 1h, wash with anhydrous ethanol 3 times, and transfer to an oven to dry to obtain a microcapsule flame retardant additive; in the above reaction, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, trifluoroacetic acid and THF is 10g:3g:0.3g:50mL:11.5g:200mL;

[0110] 2) Preparation of flame-retardant cables with high insulation

[0111] s1: 20 parts of microcapsule flame retardant additive, 0.8 parts of lubricant, 3 parts of stabilizer, 1.5 parts of antioxidant and 1.5 parts of pigment are mixed and added into a blender to prepare a functional mixture;

[0112] s2: Mix 100 parts of polyvinyl chloride resin, 30 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 150℃, 170℃, 190℃, 220℃, 220℃ and 200℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0113] Comparative Example 1

[0114] This comparative example uses the flame-retardant cross-linked polyvinyl chloride insulated cable in CN116230297A;

[0115] Comparative Example 2

[0116] The specific implementation process of preparing an insulated flame-retardant cable in this comparative example is as follows:

[0117] s1: 18 parts of microcapsule flame retardant additive (the magnesium hydroxide microcapsule flame retardant in Chinese patent CN112225945B is selected in this comparative example), 0.8 parts of lubricant, 3 parts of stabilizer, 1.5 parts of antioxidant and 1.5 parts of pigment are mixed and added into a stirrer to prepare a functional mixture;

[0118] s2: Mix 100 parts of polyvinyl chloride resin, 30 parts of plasticizer and functional mixture and feed them into a twin-screw extruder. Adjust the temperature of each zone of the twin-screw to 150℃, 170℃, 190℃, 220℃, 220℃ and 200℃, apply 80r / min, and the extrusion mass flow rate is 40kg / h. Melt blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a high-insulation flame-retardant cable.

[0119] Resistivity test:

[0120] The volume resistivity of the high-insulation flame-retardant cables prepared in Examples 1-6 and the insulation layers prepared in Comparative Examples 1-2 was tested at 20° C. in accordance with GB / T1410-2007;

[0121] Resistivity test under wet conditions:

[0122] After soaking the sample in water for 5 hours, the volume resistivity was tested according to GB / T1410-2007;

[0123] Flame retardant performance test:

[0124] The high-insulation flame-retardant cables prepared in Examples 1-6 and the insulation layers prepared in Comparative Examples 1-2 were cut into standard test specimens of 125±5 mm×13±0.5 mm and 3.2 mm thick, and flame retardant performance tests were performed in accordance with UL94.

[0125] Limiting oxygen index test: Test the test specimens in accordance with GB / T2406-2008;

[0126] Tensile strength test:

[0127] The flame-retardant cables with high insulation properties prepared in Examples 1-6 and the insulating layers prepared in Comparative Examples 1-2 were prepared into test specimens according to GB / T1040.1-2018 and tested. The test data are shown in Table 2:

[0128] Table 2

[0129]

[0130]

[0131] From the data in Table 1, it can be seen that the resistivity of the high-insulation flame-retardant cables prepared in Examples 1-6 at room temperature is 6.9-7.6X10 12 Ω.m, slightly higher than the insulated flame-retardant cables prepared in Comparative Examples 1-2. However, under the soaking condition, the resistivity of the high-insulation flame-retardant cables prepared in Examples 1-6 was 8.5-9.2X10 10 Ω.m, which is significantly higher than the insulated flame-retardant cable prepared in Comparative Example 1, and has a resistivity similar to that of the insulated flame-retardant cable prepared in Comparative Example 2. However, in terms of tensile strength, the high-insulation flame-retardant cables prepared in Examples 1-6 are significantly higher than the insulated flame-retardant cables prepared in Comparative Examples 1-2, and the high-insulation flame-retardant cables prepared in Examples 1-6 are significantly higher in flame retardant performance and limiting oxygen index than Comparative Example 1; this indicates that a high-insulation flame-retardant cable disclosed in the present invention has good insulation both at room temperature and under soaking conditions, and its flame retardant performance and tensile strength are also significantly improved.

[0132] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A flame-retardant cable with high insulation, characterized in that: The invention comprises a cable core and an insulating flame retardant protective layer on the surface thereof, wherein the insulating flame retardant protective layer comprises, by weight, 100 parts of polyvinyl chloride, 20-30 parts of plasticizer, 10-20 parts of microcapsule flame retardant additive, 0.5-0.8 parts of lubricant, 2-3 parts of stabilizer, 1-1.5 parts of antioxidant and 1-1.5 parts of pigment; The microcapsule flame retardant additive is prepared by the following method: Step A1: epichlorohydrin, boron trifluoride etherate and carbon tetrachloride are mixed and added, the temperature is raised to 60-70° C., pentaerythritol triallyl ether is added dropwise to a reaction kettle, and the mixture is refluxed and reacted at a constant temperature for 2-3 hours, and then a 25% by mass sodium hydroxide solution is added to the mixed solution, the temperature is raised to 75° C., the reaction is continued with stirring for 3 hours, and then the intermediate 1 is obtained by vacuum rotary evaporation; Step A2: DOPO, triphenylphosphine and DMF were mixed and added, the temperature was raised to 110-120°C, intermediate 1 was added dropwise to the reaction kettle, the mixture was stirred and reacted for 1-2 hours, and then washed with water for 2-3 times to remove DMF, and then transferred to an oven and dried for 5 hours to obtain intermediate 2; Step A3: diethylenetriamine, sodium ethoxide and toluene are mixed and added, the temperature is raised to 30-40°C, intermediate 2 is added dropwise to the reaction kettle, the mixture is stirred and reacted for 3-4 hours, and then vacuum rotary evaporation is performed to obtain intermediate 3; Step A4: Mix the intermediate 3, triethylamine and THF, add p-toluenesulfonyl chloride dropwise into the reaction kettle, stir at room temperature for 8-10 hours, then continue to add sodium hydroxide and propylene chloride dropwise, raise the temperature to 40-50°C, keep stirring and react for 1-2 hours, then evaporate under reduced pressure to obtain the intermediate 4; Step A5: Put the magnesium hydroxide and ethanol solution in a beaker, stir for 20 minutes, then add A174, heat to 25-30°C, stir for 2 hours, filter and wash, then transfer the filter cake to an oven and dry for 24 hours to obtain modified magnesium hydroxide; Step A6: Take intermediate 4, modified magnesium hydroxide, AIBN initiator and THF, mix and feed, heat to 50-60°C, stir and react for 4-5 hours, and then evaporate under reduced pressure to obtain a crude microcapsule flame retardant additive. Then, mix the crude product, hydrogen bromide acetic acid solution and phenol, heat to 60-70°C, stir and react for 1 hour, wash with anhydrous ethanol 2-3 times, and transfer to an oven to dry to obtain a microcapsule flame retardant additive.

2. A flame-retardant cable with high insulation according to claim 1, characterized in that: In step A1, the amount ratio of epichlorohydrin, pentaerythritol triallyl ether, boron trifluoride etherate, sodium hydroxide solution and carbon tetrachloride is 0.15 mol: 0.1 mol: 0.5-0.8 g: 15 mL: 50 mL.

3. A flame-retardant cable with high insulation according to claim 2, characterized in that: In step A2, the usage ratio of DOPO, intermediate 1, triphenylphosphine and DMF is 0.1 mol: 0.1 mol: 0.3-0.5 g: 80 mL.

4. A flame-retardant cable with high insulation according to claim 3, characterized in that: In step A3, the usage ratio of diethylenetriamine, intermediate 2, sodium ethoxide and toluene is 0.15 mol: 0.05 mol: 10-15 mL: 100 mL.

5. A flame-retardant cable with high insulation according to claim 4, characterized in that: In step A4, the usage ratio of intermediate 3, triethylamine, p-toluenesulfonyl chloride, propylene chloride, sodium hydroxide and THF is 0.02 mol: 2-2.5 g: 0.12 mol: 0.02 mol: 1-1.5 g: 150 mL.

6. A flame-retardant cable with high insulation according to claim 5, characterized in that: In step A5, the usage ratio of magnesium hydroxide, A174 and ethanol solution is 50 g: 0.5-0.8 g: 200 mL; the mass fraction of the ethanol solution is 60%.

7. A flame-retardant cable with high insulation according to claim 6, characterized in that: In step A6, the amount ratio of intermediate 4, modified magnesium hydroxide, AIBN initiator, hydrogen bromide acetic acid solution, phenol and THF is 10g: 3-5g: 0.2-0.3g: 50mL: 11.5g: 200mL.

8. A production process of a flame-retardant cable with high insulation according to claim 6, characterized in that: The steps include: Step S1: mixing a microcapsule flame retardant additive, a lubricant, a stabilizer, an antioxidant and a pigment into a stirrer to prepare a functional mixture; Step S2: Mix the polyvinyl chloride resin, plasticizer and functional mixture into a twin-screw extruder, melt-blend and extrude around the cable core, then pass the coated cable core through a thermoplastic box to obtain a protective layer, and finally cool and solidify to obtain a flame-retardant cable with high insulation.

9. The production process of the high-insulation flame-retardant cable according to claim 8, characterized in that: The lubricant is a mixture of calcium stearate and natural paraffin in a weight ratio of 1:2.