A kind of basalt fiber cloth for indoor use

Through magnetization of basalt fibers, modification of cyclohexanhexanolhexanophosphate and polyetherimide, combined with the modification of 3-aminopropyltriethoxysilane and silane coupling agent, the mechanical strength of basalt fiber materials is solved. and the problem of insufficient thermal insulation performance, high-performance basalt fiber cloth suitable for interior decoration was prepared.

CN118292268BActive Publication Date: 2024-11-08XINGAN LEAGUE SHIYUAN BASALT FIBER ENG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410415469.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-11-08
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

The existing basalt fiber materials lack effective surface modification and wetting agent combination during the preparation process, resulting in insufficient mechanical strength and thermal insulation performance, and it is difficult to meet the multiple needs of interior decoration materials.

Method used

The magnetized basalt fibers are modified by cyclohexanhexanol hexafluoric acid and polyetherimide to form a high-density connection network, and are modified by 3-aminopropyltriethoxysilane and silane coupling agent. Improve the bonding performance of fibers and wetting agents, and combine bonding processing technology to prepare basalt fiber cloth with excellent mechanical properties and thermal insulation properties.

Benefits of technology

It significantly improves the mechanical strength and thermal insulation performance of basalt fiber cloth, and is suitable for interior decoration materials, such as curtain cloth, to meet the family's light-shielding, flame retardant and thermal insulation needs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a basalt fiber cloth for indoor use, wherein the fiber cloth comprises a fiber layer and a thermal insulation layer, and the basalt fiber cloth is prepared by the following preparation method: magnetized basalt fibers are modified with cyclohexanehexanol hexaphosphate and then twisted into coarse sand, then impregnated with polyetherimide and woven into fiber cloth, then immersed in an immersion liquid, dried to obtain a fiber layer, and then a thermal insulation layer is applied on one side or both sides of the fiber layer to obtain the indoor fiber cloth, the fiber cloth has good thermal insulation performance, flame retardant performance and mechanical properties, and can be used for interior decoration materials such as curtains and drapes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a basalt fiber cloth for indoor use. Background Art

[0002] Basalt fiber has high strength and durability, and can resist wear and damage in daily use. The melting point of basalt fiber is as high as 1200-1350℃, which is not easy to burn and can effectively retard flames, thus ensuring home fire safety. There are many pores inside basalt fiber, which makes it have good thermal insulation performance and can effectively block the heat exchange between indoor and outdoor. Basalt fiber is a pure natural inorganic non-metallic material that does not contain harmful substances, can be naturally degraded, and has no pollution to the environment. It has good shading performance: basalt fiber curtains can effectively block the light exchange between indoor and outdoor, providing good shading effect. At the same time, basalt fiber is a material with excellent performance and moderate cost, which can meet the needs of most families. Summary of the invention

[0003] The present invention provides a basalt fiber cloth for indoor use, wherein the fiber cloth comprises a fiber layer and a thermal insulation layer, and the basalt fiber cloth is prepared by the following preparation method: magnetized basalt fibers are modified with cyclohexanehexanol hexaphosphate and then twisted into coarse sand, then impregnated with polyetherimide and woven into fiber cloth, then immersed in an immersion liquid, dried to obtain a fiber layer, and then a thermal insulation layer is applied on one side or both sides of the fiber layer to obtain the indoor fiber cloth, the fiber cloth has good thermal insulation performance, flame retardant performance and mechanical properties, and can be used for interior decoration materials such as curtains and drapes.

[0004] A method for preparing basalt fiber cloth, characterized in that the preparation method comprises:

[0005] 1) crushing and melting the basalt ore, pouring it into deionized water and rapidly cooling it, and then crushing and melting it again to form a spinning melt; drawing the spinning melt to obtain basalt fiber precursor;

[0006] 2) immersing the basalt fiber precursor in an ethanol solution of 3-aminopropyltriethoxysilane, heating for a predetermined time, taking out and drying; then placing in a cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersing, immersing, taking out and drying;

[0007] 3) twisting the basalt fiber obtained in step 2) into coarse sand, and then soaking it in an ethanol solution of polyetherimide; taking it out and drying it, and then weaving it into a fiber cloth;

[0008] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid, taking it out and drying it to obtain a modified basalt fiber mesh cloth;

[0009] 5) Apply a thermal insulation layer on one or both sides of the modified basalt fiber mesh cloth to obtain the product.

[0010] Furthermore, in step 1: the basalt ore is crushed, melted at 1400-1500°C, then poured into deionized water and rapidly cooled, then crushed again, and melted at 1300-1350°C to form a spinning melt.

[0011] Furthermore, in step 2, the basalt fiber precursor is immersed in a 20-25wt% 3-aminopropyltriethoxysilane ethanol solution, heated at 60-80°C for a predetermined time, and taken out to dry; then placed in a 0.1-0.2wt% cyclohexanehexol hexaphosphate aqueous solution, ultrasonically dispersed, immersed, and taken out to dry.

[0012] Furthermore, in step 3: the coarse sand is immersed in a 1-2 wt % polyetherimide ethanol solution.

[0013] Furthermore, in step 3, the plurality of basalt fibers obtained in step 2 are twisted into one strand by a stranding machine, wherein the linear density of the coarse sand is 1500-4000 tex and the gram weight of the fiber cloth is 400±5 g·m -2 ; Warp and weft density: 30×28 / root·cm -1 .

[0014] Furthermore, in step 4, the impregnation liquid includes: the impregnation liquid includes: 10-15wt% of water-based epoxy resin, 5-6wt% of water-based polyurethane, 0.5-1wt% of silane coupling agent KH-560 and the balance of deionized water.

[0015] Furthermore, the step 5 is to mix 1-2wt% of carbon black, 10-15wt% of antimony trioxide, 0.5-1wt% of aluminum trioxide, and the rest of PET, add the materials into a screw extruder, extrude, cool and shape, and obtain a sheet-like film with a thickness of 10-20 microns, which is bonded to the cloth through bonding. The bonding resin used is a polyurethane and epoxy resin with a mass ratio of 1:1, and the usage amount is 5-10g / m 2 .

[0016] Furthermore, a basalt fiber cloth is provided, and the fiber cloth is obtained by the preparation method.

[0017] Furthermore, an indoor fabric is provided, wherein the indoor fabric comprises basalt fiber fabric.

[0018] Beneficial technical effects of the present invention

[0019] 1) In the process of preparing basalt fiber, the present invention uses cold water rapid quenching to make the basalt fiber have partial magnetism, thereby improving the effect of surface modification;

[0020] 2) Before weaving, the basalt fiber is modified with 3-aminopropyl triethoxysilane, cyclohexane hexaphosphate and amino polymer to form a high-density connection network, which can improve the wettability and bonding performance between the basalt fiber and the water-based epoxy resin in the sizing agent, thereby improving the mechanical strength of the basalt fiber cloth;

[0021] 3) The sizing agent of the present invention contains silane coupling agent KH-550, polyoxyethylene stearate, polyvinyl acetate and water-based polyurethane, which can quickly graft a large number of active groups on the fiber surface, improve the mechanical properties of basalt fiber, and at the same time improve the chemical bonding ability between basalt fiber and insulation layer. DETAILED DESCRIPTION

[0022] The present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples within the scope not exceeding the gist of the present invention.

[0023] Example 1

[0024] 1) The basalt ore is crushed, melted at 1400°C, poured into 0°C deionized water and rapidly cooled, then crushed again, melted at 1300°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0025] 2) immersing the basalt fiber precursor in a 20wt% 3-aminopropyltriethoxysilane ethanol solution, heating at 60°C for 1 hour, taking out and drying; then placing in a 0.1wt% cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersing, immersing for 30 minutes, taking out and drying;

[0026] 3) The basalt fiber obtained in step 2) is twisted into a strand of coarse sand using a stranding machine, wherein the linear density of the coarse sand is 2000 tex, and then placed in a 1wt% ethanol solution of polyetherimide for 30 minutes; taken out and dried, and then woven into a fiber cloth, wherein the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0027] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0028] 5) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0029] Example 2

[0030] 1) The basalt ore is crushed, melted at 1500°C, then poured into 0°C deionized water and rapidly cooled, then crushed again, and melted at 1350°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0031] 2) immersing the basalt fiber precursor in a 25wt% 3-aminopropyltriethoxysilane ethanol solution, heating at 80°C for 1h, taking out and drying; then placing in a 0.2wt% cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersing, immersing for 30min, taking out and drying;

[0032] 3) The basalt fiber obtained in step 2) is twisted into a strand of coarse sand using a stranding machine, wherein the linear density of the coarse sand is 2000 tex, and then placed in a 2wt% ethanol solution of polyetherimide for 30 minutes; taken out and dried, and then woven into a fiber cloth, wherein the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0033] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 15wt% of water-based epoxy resin, 6wt% of water-based polyurethane, 1wt% of silane coupling agent KH-560 and the balance of deionized water;

[0034] 5) 2wt% carbon black, 15wt% antimony trioxide, 1wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0035] Example 3

[0036] 1) The basalt ore is crushed, melted at 1450°C, poured into 0°C deionized water and rapidly cooled, then crushed again, melted at 1300°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0037] 2) immersing the basalt fiber precursor in a 22wt% 3-aminopropyltriethoxysilane ethanol solution, heating at 70°C for 1h, taking out and drying; then placing in a 0.1wt% cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersing, immersing for 30min, taking out and drying;

[0038] 3) The basalt fiber obtained in step 2) is twisted into a strand of coarse sand using a stranding machine, wherein the linear density of the coarse sand is 2000 tex, and then placed in a 2wt% ethanol solution of polyetherimide for 30 minutes; taken out and dried, and then woven into a fiber cloth, wherein the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0039] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 12wt% of waterborne epoxy resin, 6wt% of waterborne polyurethane, 1wt% of silane coupling agent KH-560 and the balance of deionized water;

[0040] 5) 2wt% carbon black, 15wt% antimony trioxide, 1wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0041] Comparative Example 1

[0042] 1) crushing basalt ore and melting it at 1300°C to form a spinning melt; drawing the spinning melt to obtain basalt fiber precursor with a diameter of 100 microns;

[0043] 2) The obtained basalt fiber is twisted into a strand using a stranding machine, wherein the linear density of the coarse sand is 2000 tex, and then woven into a fiber cloth, wherein the gram weight of the fiber cloth is 400±5 g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0044] 3) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0045] 4) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0046] Comparative Example 2

[0047] 1) The basalt ore is crushed, melted at 1400°C, poured into 0°C deionized water and rapidly cooled, then crushed again, melted at 1300°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0048] 2) The obtained basalt fiber is twisted into a strand using a stranding machine, wherein the linear density of the coarse sand is 2000 tex, and then woven into a fiber cloth, wherein the gram weight of the fiber cloth is 400±5 g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0049] 3) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0050] 4) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0051] Comparative Example 3

[0052] 1) crushing basalt ore and melting it at 1300°C to form a spinning melt; drawing the spinning melt to obtain basalt fiber precursor with a diameter of 100 microns;

[0053] 2) immersing the basalt fiber precursor in a 20wt% 3-aminopropyltriethoxysilane ethanol solution, heating at 60°C for 1 hour, taking out and drying; then placing in a 0.1wt% cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersing, immersing for 30 minutes, taking out and drying;

[0054] 3) The basalt fiber obtained in step 2) is twisted into a strand by a stranding machine, wherein the linear density of the coarse sand is 2000 tex, and then placed in a 1wt% polyetherimide ethanol solution for soaking for 30 minutes; taken out and dried, and then woven into a fiber cloth, wherein the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0055] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0056] 5) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0057] Comparative Example 4

[0058] 1) The basalt ore is crushed, melted at 1400°C, poured into 0°C deionized water and rapidly cooled, then crushed again, melted at 1300°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0059] 2) immersing the basalt fiber precursor in a 20 wt % 3-aminopropyltriethoxysilane ethanol solution, heating at 60° C. for 1 h, and taking out to dry;

[0060] 3) twisting the basalt fiber obtained in step 2) into coarse sand, and then soaking it in a 1wt% polyetherimide ethanol solution for 30 minutes; taking it out and drying it, twisting it into a strand using a stranding machine, wherein the linear density of the coarse sand is 2000tex, and then weaving it into a fiber cloth, the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0061] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0062] 5) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0063] Comparative Example 5

[0064] 1) The basalt ore is crushed, melted at 1400°C, poured into 0°C deionized water and rapidly cooled, then crushed again, melted at 1300°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0065] 2) The basalt fiber is twisted into a strand by a stranding machine, wherein the linear density of the coarse sand is 2000 tex, immersed in a 20wt% 3-aminopropyltriethoxysilane ethanol solution, heated at 60°C for 1 hour, and taken out to dry; then placed in a 0.1wt% cyclohexane hexaphosphate aqueous solution, ultrasonically dispersed, immersed for 30 minutes, taken out to dry, and then placed in a 1wt% polyetherimide ethanol solution for 30 minutes; taken out and dried, and then woven into a fiber cloth, the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0066] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0067] 5) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0068] Comparative Example 6

[0069] 1) The basalt ore is crushed, melted at 1400°C, poured into 0°C deionized water and rapidly cooled, then crushed again, melted at 1300°C to form a spinning melt; the spinning melt is drawn to obtain basalt fiber precursors with a diameter of 100 microns;

[0070] 2) Immerse the raw silk in a 20wt% 3-aminopropyltriethoxysilane ethanol solution, heat at 60°C for 1h, take out and dry; then place it in a 0.1wt% cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically disperse, immerse for 30min, take out and dry, then place it in a 1wt% polyetherimide ethanol solution and soak for 30min; take it out and dry, twist it into a strand using a stranding machine, wherein the linear density of the coarse sand is 2000tex, and then weave it into a fiber cloth, the gram weight of the fiber cloth is 400±5g·m -2 ; Warp and weft density: 30×28 / root·cm -1 ;

[0071] 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid for 30 minutes, taking it out and drying it to obtain a modified basalt fiber mesh cloth, wherein the impregnation liquid comprises: 10wt% of water-based epoxy resin, 5wt% of water-based polyurethane, 0.5wt% of silane coupling agent KH-560 and the balance of deionized water;

[0072] 5) 1wt% carbon black, 10wt% antimony trioxide, 0.5wt% aluminum trioxide, and the rest PET are mixed evenly, added to a screw extruder, extruded, cooled and shaped to obtain a 10-micron-thick sheet film, which is bonded to the fabric by bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5g / m 2 .

[0073] Experimental results

[0074] The tear strength of the fabric prepared was tested according to GB / T3923.2-2013 standard, as shown in Table 1.

[0075] Table 1

[0076] Tear strength (warp direction, unit N) Tear strength (weft direction, unit N) Example 1 268 245 Example 2 272 250 Example 3 265 242 Comparative Example 1 215 196 Comparative Example 2 213 192 Comparative Example 3 252 230 Comparative Example 4 235 203 Comparative Example 5 248 221 Comparative Example 6 242 217

[0077] It can be seen from the data of the embodiments and comparative examples that in the process of preparing basalt fiber, the present invention uses cold water quenching to make the basalt fiber partially magnetic, which can improve the effect of fiber surface modification and has a positive effect on improving the strength of the fiber cloth; the basalt fiber is modified with 3-aminopropyl triethoxysilane, cyclohexane hexaphosphate and amino polymer before weaving, and a high-density connection network can be formed between the three components, which can improve the wettability and bonding performance between the basalt fiber and the sizing agent, thereby improving the mechanical strength of the basalt fiber cloth; at the same time, the applicant found that after soaking in cyclohexane hexaphosphate before twisting, surface modification with polyetherimide after twisting can improve the strength of the fiber cloth. The reason may be that if the modification process is carried out before twisting, the rough structure formed on the surface of the basalt fiber raw silk is not conducive to the twisting process, and soaking after twisting is likely to lead to insufficient soaking, affecting the effect of the modification process.

[0078] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention.

Claims

1. A method for preparing basalt fiber cloth, It is characterized in that The preparation method comprises: 1) crushing and melting the basalt ore, pouring it into deionized water and rapidly cooling it, and then crushing and melting it again to form a spinning melt; drawing the spinning melt to obtain basalt fiber precursor; 2) immersing the basalt fiber precursor in an ethanol solution of 3-aminopropyltriethoxysilane, heating for a predetermined time, taking out and drying; then placing in a cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersing, immersing, taking out and drying; 3) twisting the basalt fiber obtained in step 2) into roving, and then soaking it in an ethanol solution of polyetherimide; taking it out and drying it, and then weaving it into a fiber cloth; 4) immersing the basalt fiber cloth obtained in step 3) in an impregnation liquid, taking it out and drying it to obtain a modified basalt fiber mesh cloth; 5) Apply a thermal insulation layer on one or both sides of the modified basalt fiber mesh cloth to obtain the product.

2. The preparation method according to claim 1, It is characterized in that In step 1), the basalt ore is crushed, melted at 1400-1500° C., poured into deionized water and rapidly cooled, and then crushed again and melted at 1300-1350° C. to form a spinning melt.

3. The preparation method according to claim 1, It is characterized in that In step 2), the basalt fiber precursor is immersed in a 20-25wt% 3-aminopropyltriethoxysilane ethanol solution, heated at 60-80°C for a predetermined time, and taken out to dry; then placed in a 0.1-0.2wt% cyclohexanehexol hexaphosphoric acid aqueous solution, ultrasonically dispersed, immersed, and taken out to dry.

4. The preparation method according to claim 1, It is characterized in that In step 3), the roving is immersed in a 1-2 wt % polyetherimide ethanol solution.

5. The preparation method according to claim 1, It is characterized in that In step 3), a plurality of basalt fibers obtained in step 2) are twisted into a strand by a stranding machine, wherein the linear density of the roving is 1500-4000 tex and the gram weight of the fiber cloth is 400±5 g·m -2 ; Warp and weft density: 30×28 / root·cm -1 .

6. The preparation method according to claim 1, It is characterized in that In step 4), the impregnation liquid comprises: 10-15wt% of water-based epoxy resin, 5-6wt% of water-based polyurethane, 0.5-1wt% of silane coupling agent KH-560 and the balance of deionized water.

7. The preparation method according to claim 1, It is characterized in that The step 5) is to mix 1-2wt% of carbon black, 10-15wt% of antimony trioxide, 0.5-1wt% of aluminum trioxide, and the rest of PET, add the materials into a screw extruder, extrude, cool and shape, and obtain a sheet film with a thickness of 10-20 microns, which is bonded to the cloth through bonding. The bonding resin used is polyurethane and epoxy resin in a mass ratio of 1:1, and the usage amount is 5-10g / m 2 .

8. A basalt fiber cloth, It is characterized in that The fiber cloth is obtained by the preparation method according to any one of claims 1 to 7.

9. An indoor fabric, comprising the basalt fiber fabric according to claim 8.