A kind of conductive concrete pole material without steam curing and its preparation method
By using conductive carbon black, stainless steel fiber, graphite tailings and magnetic fly ash in concrete poles, and using the power-on-free steam-free curing process, the problems of the conductive properties and production costs of existing concrete poles are solved, and the problem of conductive properties and production costs of existing concrete poles is achieved. Efficient and economical concrete pole material preparation.
Patent Information
- Application Number
- CN202410413201.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The existing concrete poles have shortcomings in terms of electrical conductivity and production costs, and the traditional steam maintenance process consumes high energy, has long cycles and is expensive.
Using mixed conductive blends, including conductive carbon black, stainless steel fiber, graphite tailings and magnetic fly ash, high conductivity and reduced production through the preparation method of modified conductive carbon black and the power-on-free steam-free maintenance process. Cost concrete pole material.
The high conductivity and good mechanical properties of concrete poles are achieved, while reducing production costs and energy consumption and improving production efficiency.
Smart Images

Figure BDA0004779913330000091 
Figure BDA0004779913330000101 
Figure BDA0004779913330000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete preparation, in particular to an energized steam-free conductive concrete pole material and a preparation method thereof. Background Art
[0002] With the development of economy and the acceleration of urbanization, power supply has become one of the indispensable infrastructures for production and life in modern society. As an important part of power transmission lines, concrete poles play an important role in the construction of power transmission lines.
[0003] Existing concrete poles mainly improve the conductivity of concrete by adding a small amount (less than 1%) of conductive steel fiber or carbon fiber to the concrete. However, the price of carbon fiber is relatively high, and the resistivity of the prepared conductive concrete is relatively high, so it is not suitable for large-scale use. In addition, traditional concrete poles usually use steam curing technology, that is, high temperature and high humidity environment conditions are used for curing during the concrete curing process to accelerate the hardening of the concrete and improve the strength of the material. However, the steam curing process has problems such as high energy consumption, long cycle, and high cost, which is not conducive to energy conservation and emission reduction and reducing production costs. Summary of the invention
[0004] The purpose of the present invention is to provide an energized, steam-curing-free conductive concrete pole material and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is a mixed conductive admixture, comprising the following raw materials in parts by weight: 15 to 25 parts of conductive carbon black, 25 to 39 parts of magnetic fly ash, 15 to 26 parts of crude steel slag, 5 to 15 parts of stainless steel fiber and 15 to 25 parts of graphite tailings.
[0007] Furthermore, the mixed conductive admixture also includes 30 to 40 parts of modified conductive carbon black.
[0008] Furthermore, the preparation method of the modified conductive carbon black comprises the following steps:
[0009] Conductive carbon black is ultrasonically dispersed in water, then ozone is introduced and stirred for reaction to obtain oxidized carbon black;
[0010] The aramid fiber is soaked in a sulfuric acid solution and then soaked in a sodium bicarbonate solution to obtain a pretreated aramid fiber;
[0011] The pretreated aramid fiber is added into a mixed solution of oxalyl chloride and dichloromethane, and heated to react to obtain chlorinated aramid fiber;
[0012] The oxidized carbon black and the chlorinated aramid fiber are added into an organic solvent and heated to undergo reflux reaction to obtain the modified conductive carbon black.
[0013] Furthermore, the mass ratio of the conductive carbon black to water is 1:10; the flow rate of the ozone is 60-80 mL / min; the stirring reaction time is 15-20 h;
[0014] The concentration of the sulfuric acid solution is 25-30wt.%; the aramid fiber is immersed in the sulfuric acid solution for 30-40 minutes; the concentration of the sodium bicarbonate solution is 0.5wt.%; the aramid fiber is immersed in the sodium bicarbonate solution for 4-5 minutes.
[0015] Furthermore, the amount ratio of the pretreated aramid fiber, oxalyl chloride and dichloromethane is 1g:5mL:10mL; the temperature of the heating reaction is 60-65°C, and the time is 10-12h;
[0016] The mass ratio of the oxidized carbon black to the chlorinated aramid fiber is 5:1; and the heating reflux reaction time is 8 to 10 hours.
[0017] The second technical solution of the present invention: an energized steam-free conductive concrete pole material, the raw materials comprising: 15 parts by mass of the above-mentioned mixed conductive admixture, 12-20 parts by mass of cement, 23-35 parts by mass of sand, 25-44 parts by mass of crushed stone, 8-20 parts by mass of water and concrete admixture;
[0018] The dosage of the concrete admixture is 2.1% of the mass of cement.
[0019] Furthermore, the concrete admixture consists of hydroxyethyl cellulose, polycarboxylate high-efficiency water reducing agent, organosilicon defoaming agent and calcium formate early strength agent in a mass ratio of 0.4:1:0.2:0.5.
[0020] The third technical solution of the present invention is a method for preparing the above-mentioned conductive concrete pole material without steam curing, comprising the following steps:
[0021] The stainless steel fiber, the concrete admixture and 1 / 2 water are mixed and stirred evenly to obtain a mixture 1;
[0022] Adding sand, gravel and crude steel slag to mixture 1 and stirring evenly to obtain mixture 2;
[0023] Adding graphite tailings, magnetic fly ash and cement to mixture 2, adding the remaining water after mixing evenly, stirring evenly, to obtain mixture 3;
[0024] Other raw materials are added to the mixture 3 and stirred evenly to obtain the electrification-free steam-curing conductive concrete pole material.
[0025] Technical solution 4 of the present invention: Application of the above-mentioned energized and steam-free conductive concrete pole material in power supply.
[0026] As a new type of industrial material, stainless steel fiber has excellent properties such as high conductivity, high thermal conductivity, high strength, high temperature resistance, and corrosion resistance. It also has the characteristics of chemical fiber and synthetic fiber, and is widely used in many industrial fields such as petroleum, chemical industry, and electronics. The conductivity of stainless steel fiber is far better than that of carbon fiber, and its resistivity is extremely low. Therefore, it can be used in the preparation of conductive concrete. In addition, stainless steel fiber is completely resistant to corrosion by nitric acid, phosphoric acid, alkali and organic solutions, and has strong corrosion resistance to sulfate ions and chloride ions, so it is very suitable for the internal environment of concrete. In a high temperature aerobic environment, stainless steel fiber can be used continuously and has good heat resistance. At room temperature, its breaking strength is between 686 and 980 MPa, with high relative strength and good wear resistance. These characteristics make stainless steel fiber an excellent material for preparing conductive concrete.
[0027] Conductive carbon black is a conductive material with high specific surface area, excellent conductivity and high purity. Conductive carbon black has a relatively low preparation cost, so it is widely used in the preparation of conductive products, antistatic products and composite polymer materials. Adding a proper amount of carbon black particles can improve the compressive strength and toughness of conductive cement-based composite materials. Adding more carbon black particles can achieve the ideal resistivity, but too much carbon black particles will reduce the fluidity, density and compressive strength of cement.
[0028] Steel slag (crude steel slag) is a by-product of the steelmaking process. It is composed of various oxides formed by the oxidation of impurities in pig iron (such as silicon, manganese, phosphorus, sulfur, etc.) during the smelting process, as well as salts generated by the reaction of these oxides with solvents. The use of steel slag in concrete can replace part of the aggregate, reduce the cost of concrete and reduce the negative impact on the environment; it can improve the strength, impermeability, carbonation resistance and durability of concrete; and steel slag can also improve the fluidity, consistency and slump of concrete, further optimizing the working performance of concrete. Therefore, the use of steel slag in concrete is of great significance for improving the performance of concrete and reducing production costs.
[0029] Graphite tailings are solid wastes generated in large quantities during graphite mining. Every ton of graphite mined will produce 10 to 15 tons of graphite tailings. The large accumulation of graphite tailings reduces land utilization, leading to environmental deterioration and soil erosion around the mining area. In addition, the particles of graphite tailings are small, which can easily cause sand blowing and cause serious damage to the ecological environment. Studies have shown that graphite tailings can replace natural sand in concrete production to produce concrete with higher mechanical properties. At the same time, the addition of graphite tailings can reduce the resistivity of concrete. However, due to the limited graphite content in graphite tailings, adding graphite tailings alone cannot effectively reduce the resistivity, so other conductive materials need to be added to improve the conductivity of concrete.
[0030] Magnetic fly ash is a special type of fly ash obtained by extracting iron oxides from ordinary fly ash using a magnetic separation process. The magnetic separation process can effectively separate iron oxides from fly ash, significantly increasing the content of iron oxides Fe3O4 in magnetic fly ash. This high-iron content magnetic fly ash has excellent electrical conductivity and shows unique advantages in the application of conductive concrete. The reuse of magnetic fly ash not only helps to reduce the emission of solid waste, but also reduces production costs and improves resource utilization efficiency, with significant economic and environmental benefits.
[0031] Although a single conductive material can meet the conductive performance requirements of conductive concrete, it has problems such as low mechanical properties, high preparation cost and poor resistivity stability. The present invention can simultaneously exert the characteristics of several conductive materials by compounding multiple conductive phase materials, play a role of mutual compensation and mutual promotion, give full play to the long- and short-range effects of each material, and form a continuous conductive path in the concrete, thereby enhancing the conductivity and mechanical properties of the concrete (stronger than the conductive performance of a single material); and the compounding of multiple conductive phase materials can significantly reduce the preparation cost of conductive concrete.
[0032] Hydroxyethyl cellulose (HEC) can effectively solve the problems of fiber agglomeration and flake formation during the mixing process, thereby ensuring the uniform dispersion of the fibers in the concrete. At the same time, hydroxyethyl cellulose can be combined with other conductive materials to form an electronic conductive path, which helps to effectively reduce the resistance of the concrete.
[0033] Organosilicon defoamers can reduce the porosity of concrete, improve the density and strength of concrete, and improve the appearance quality of concrete, reduce surface defects and pores, make the concrete surface smoother and more uniform, which is beneficial to improve the durability of concrete, reduce permeability, and enhance the anti-seepage and anti-freeze-thaw properties; and organosilicon defoamers can also improve the fluidity of concrete, which is beneficial to construction operations.
[0034] Polycarboxylate high-efficiency water reducer can significantly reduce the water-cement ratio of concrete, so that the concrete has higher compressive strength and tensile strength, and can also improve the fluidity and pumpability of concrete, reduce the pore structure inside the concrete, and facilitate the pouring and construction of concrete. In addition, polycarboxylate high-efficiency water reducer can reduce the amount of cement to a certain extent, reduce the cost of concrete, and improve the performance of concrete, achieving the goals of economic, environmental and sustainable development.
[0035] Calcium formate early strength agent can accelerate the setting and hardening process, improve the early strength and crack resistance of concrete, shorten the setting and hardening time of concrete, and improve construction efficiency; using it in appropriate amounts can achieve the ideal early strength effect.
[0036] After the conductive carbon black and chlorinated aramid fiber are grafted, the conductive carbon black surface can have active groups, which can then cross-link with other raw materials to form a three-dimensional network structure, thereby improving the density and strength of the material; at the same time, the conductive carbon black can be modified to avoid the problem of carbon black agglomerating together and affecting fluidity. Therefore, the conductive carbon black can be modified (modified conductive carbon black) to avoid the problem of reduced fluidity, density and compressive strength of cement caused by excessive addition of carbon black particles, increase the amount of conductive carbon black added to cement, reduce the resistivity of cement, and the modified conductive carbon black can further improve the compressive strength of cement.
[0037] The present invention discloses the following technical effects:
[0038] (1) The mixed conductive admixture of the present invention can form a continuous conductive path in concrete, thereby enhancing the conductivity and mechanical properties of the concrete, and can significantly reduce the preparation cost of the conductive concrete.
[0039] (2) The conductive concrete pole material of the present invention does not require traditional steam curing. Concrete curing can be achieved by simply applying power, which significantly reduces the energy consumption and production cycle of preparing concrete pole materials, reduces the production cost of concrete pole materials, improves production efficiency, and is conducive to improving the competitiveness of production enterprises.
[0040] The energized steam-curing-free conductive concrete pole material of the present invention is more economical and practical, and has important application value in the construction of power transmission lines.
[0041] (3) The mixed conductive admixtures used in the present invention include components such as conductive carbon black, stainless steel fibers, graphite tailings and magnetic fly ash, all of which are highly corrosion-resistant materials. These materials are not affected by chloride ion or sulfate ion corrosion (have good corrosion resistance) and have a longer life cycle, so the human resources and costs required for maintenance can be further reduced. At the same time, the use of the mixed conductive admixtures of the present invention can give full play to the long- and short-range effects of each material, forming a continuous conductive path in the concrete, thereby enhancing the conductivity of the concrete. In addition, the addition of concrete admixtures can further improve the performance of concrete, making it more suitable for various engineering application environments. Under the joint action of the mixed conductive admixtures and concrete admixtures, the conductivity and performance of concrete are significantly improved, thereby improving the quality and sustainability of concrete poles.
[0042] (4) The energized, steam-free concrete pole material of the present invention has good electrical and mechanical properties. DETAILED DESCRIPTION
[0043] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0044] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0047] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0048] The “parts” described in the following examples are all “parts by mass”.
[0049] The raw materials used in the present invention are as follows:
[0050] (1) The particle size of conductive carbon black was 40 nm and was purchased from Hebei Moyu Chemical Co., Ltd.
[0051] (2) The particle size of magnetic fly ash is 10-20 μm, and its chemical composition is as follows:
[0052] Table 1 Chemical composition of magnetic fly ash (wt.%)
[0053] Element CaO <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> <![CDATA[Al2O3]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> <![CDATA[K2O]]> <![CDATA[SO3]]> Impurities content 2.57 25.03 52.75 12.21 0.78 1.71 0.52 0.62 3.81
[0054] (3) The particle size of crude steel slag is 2-5 mm, and the chemical composition is as follows:
[0055] Table 2 Chemical composition of crude steel slag (wt.%)
[0056] Element CaO <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> <![CDATA[Al2O3]]> MgO MnO <![CDATA[P2O5]]> <![CDATA[SO3]]> Impurities content 38.25 14.23 32.41 1.02 6.52 2.13 1.50 0.11 3.83
[0057] (4) The stainless steel fiber has a diameter of 40 μm, a length of 12 mm, and a tensile strength of 1000 MPa and was purchased from Shandong Taicheng Fiber Co., Ltd.
[0058] (5) The particle size of graphite tailings is ≤2.35mm, and the chemical composition is as follows:
[0059] Table 3 Chemical composition of graphite tailings (wt.%)
[0060] Element CaO <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> <![CDATA[Al2O3]]> <![CDATA[SO3]]> <![CDATA[K2O]]> graphite Impurities content 11.58 49.52 9.04 13.23 5.42 3.51 2.01 5.69
[0061] (6) The cement is silicate cement P·O 42.5.
[0062] (7) The particle size of sand is 0.085 to 2.0 mm.
[0063] (8) The particle size of the crushed stone is 6 to 10 mm.
[0064] The concrete of the present invention does not undergo conventional steam curing, and only requires electricity to be supplied during the curing process.
[0065] The specific method of electrification is: copper sheets are attached to both ends of the concrete material and fixed with conductive tape. Conductive silver paste is applied between the concrete and the copper plate to ensure that the two have proper circuit connection. The electrification curing time is 12 hours in total. First, the concrete is electrified for 4 hours with a constant power of 30W to ensure the basic strength of the concrete in the initial stage of curing and prevent excessive free water evaporation caused by high temperature. Then, the concrete is electrified for 8 hours with a constant power of 40W to promote the hydration reaction inside the concrete. After the electrification is completed, the concrete is transferred to a standard curing environment at room temperature for curing for 28, 56, and 112 days to obtain the electrified steam-free conductive concrete pole material.
[0066] Example 1
[0067] A method for preparing an electrified and steam-free conductive concrete pole material:
[0068] The components in Table 4 and Table 5 are used as raw materials to prepare the conductive concrete pole material without steam curing, as follows:
[0069] Table 4 Concrete with different mass proportions
[0070]
[0071] The mass proportions of conductive admixtures corresponding to the concrete of each serial number are shown in Table 2.
[0072] Table 5 Mass proportion of mixed conductive admixtures
[0073] Serial number Conductive carbon black Stainless steel fiber Crude steel slag Magnetic separation fly ash powder Graphite tailings 1 15 5 26 39 15 2 15 10 22 38 15 3 15 15 20 35 15 4 20 5 26 29 20 5 20 10 22 28 20 6 20 15 20 25 20 7 25 5 15 30 25 8 15 5 26 39 15
[0074] Serial numbers 1 to 8 represent 8 different types of concrete.
[0075] The preparation method of the concrete of No. 1 to 7 is as follows:
[0076] (1) Stainless steel fiber, concrete admixture and 1 / 2 water are mixed and stirred using a mixer until no obvious lumps or flakes remain, thereby obtaining a mixture 1;
[0077] (2) adding sand, gravel and crude steel slag to mixture 1, and stirring for 30 seconds using a mixer to obtain mixture 2;
[0078] (3) adding graphite tailings, magnetic fly ash and cement to mixture 2, mixing evenly, adding the remaining water, and stirring for 60 seconds to obtain mixture 3;
[0079] (4) Add conductive carbon black to mixture 3 and stir for about 100 seconds. When the concrete has good workability, the stirring is completed to obtain a conductive concrete pole material that is energized and does not require steaming.
[0080] The preparation method of the concrete of No. 8 is as follows:
[0081] (1) Pour stainless steel fiber, sand, gravel and crude steel slag into a mixer and dry mix for 30 seconds.
[0082] (2) Pour 1 / 2 of the water into the mixer and stir for 30 seconds, then pour in the graphite tailings, magnetic fly ash powder and cement and stir for 60 seconds.
[0083] (3) Add conductive carbon black to the reaction system of step (2), and add the remaining water, stir for about 100 seconds, and complete the stirring when the concrete has good workability, thereby obtaining a conductive concrete pole material.
[0084] According to the requirements of the concrete centrifugal forming process, the slump of the prepared concrete must be between 40 and 80 mm; and the compressive strength must be no less than 40 MPa to meet the requirements of the "Ring Concrete Poles" specification. Therefore, the concrete prepared by the present invention was subjected to compressive strength (reference standard GB / T11837-2009, without traditional steam curing, and powered on, the specific method is: copper sheets are attached to both ends of the concrete material, and are fixed with conductive tape, and conductive silver paste is coated between the concrete and the copper plate to ensure that the two have proper circuit connection, and the power-on curing time is 12 hours in total. First, the concrete is powered on for 4 hours at a constant power of 30W to ensure the basic strength of the concrete in the initial stage of curing and prevent excessive free water evaporation caused by high temperature, and then the concrete is continuously powered on for 8 hours at a constant power of 40W to promote the hydration reaction inside the concrete. After the power-on is completed, the concrete is transferred to a standard curing environment at room temperature and cured to 28d, 56d, and 112d to obtain a conductive concrete pole material powered on and steam-free. The results are shown in Table 6.
[0085] Table 6 Compressive strength and slump of concrete No. 1 to 8
[0086]
[0087]
[0088] As can be seen from Table 6, the concrete prepared by No. 1 to 7 meets the requirements of slump (between 40 and 80 mm) and compressive strength (not less than 40 Mpa). The present invention adopts a combination of multiple materials to produce conductive concrete, which can adapt to different environmental conditions. In high-cold areas or extremely arid areas, the proportion and amount of mixed conductive admixtures can be adjusted according to actual conditions to ensure that the conductive concrete can adapt to the local climate environment and engineering requirements. In addition, the concrete of the present invention has high early strength, does not require traditional steam curing, can reduce energy consumption, and speed up the construction process.
[0089] The resistivity data of different concretes are shown in Table 7.
[0090] Table 7 Resistivity of concrete No. 1 to 8
[0091] Serial number Experimental Project 28d 56d 112d 1 Resistivity / Ω·m 53.1 57.7 69.0 2 Resistivity / Ω·m 18.9 22.5 28.6 3 Resistivity / Ω·m 45.3 50.0 66.4 4 Resistivity / Ω·m 38.4 46.7 50.1 5 Resistivity / Ω·m 10.6 17.4 19.0 6 Resistivity / Ω·m 40.1 49.4 57.0 7 Resistivity / Ω·m 36.8 40.7 43.8 8 Resistivity / Ω·m 86.3 103.4 118.7
[0092] When the amount of stainless steel fiber added is high (concrete No. 3 and 6), the fiber will clump in large quantities in the concrete and cannot be effectively dispersed to form a fiber skeleton, which will cause the conductive material to be unable to form a conductive loop and the resistivity will increase to a certain extent. At the same time, the clumped stainless steel fiber in the concrete is equivalent to the presence of impurities, which will slightly reduce the mechanical properties of the concrete such as compressive strength.
[0093] Concrete No. 8 is the control group without any admixtures. Due to the lack of hydroxyethyl cellulose, the stainless steel fibers will agglomerate on a large scale inside the concrete and fail to form a conductive skeleton, resulting in increased resistivity and decreased mechanical strength. The lack of silicone defoaming agent and calcium formate early strength agent will lead to the formation of bubbles in the concrete, affecting the density of the concrete and reducing the compressive strength. The lack of water reducer will amplify the water absorption disadvantage of conductive carbon black, causing serious water shortage in the concrete and a sharp drop in fluidity, making it unable to meet construction needs.
[0094] Although the addition of conductive carbon black can enhance the conductivity of concrete, its own characteristics will affect the compressive strength of concrete. For example, the amount of conductive carbon black added to the concrete of No. 7 is the largest, resulting in the 28d compressive strength of the concrete being reduced to 41.2Mpa, which is the lowest value among all groups except the control group.
[0095] Example 2
[0096] A method for preparing an electrified and steam-free conductive concrete pole material:
[0097] The same as No. 2 in Example 1, except that the mixed conductive admixture further contains 30 parts by mass of modified conductive carbon black; the modified conductive carbon black and the conductive carbon black are added together during preparation.
[0098] Preparation method of modified conductive carbon black:
[0099] A. Ultrasonic dispersion of conductive carbon black in water (mass ratio of conductive carbon black to water is 1:10), then introduction of ozone (ozone flow rate is 70 mL / min), stirring reaction for 20 h, and obtaining oxidized carbon black.
[0100] B. adding the aramid fiber to a 25wt.% sulfuric acid solution and soaking it for 40 minutes, then adding it to a 0.5wt.% sodium bicarbonate solution and soaking it for 4 minutes, taking it out, washing it with water, and drying it to obtain the pretreated aramid fiber;
[0101] C. Add the pretreated aramid fiber to a mixed solution of oxalyl chloride and dichloromethane (the amount ratio of the pretreated aramid fiber, oxalyl chloride and dichloromethane is 1 g: 5 mL: 10 mL), heat the reaction (temperature is 65 ° C, time is 12 h), and obtain chlorinated aramid fiber;
[0102] D. Add oxidized carbon black and chlorinated aramid fiber (the mass ratio of oxidized carbon black to chlorinated aramid fiber is 5:1) into N,N-dimethylformamide, heat and reflux for 10 hours to obtain modified conductive carbon black.
[0103] Example 3
[0104] The same as Example 2, except that the mixed conductive admixture further contains 40 parts by mass of modified conductive carbon black.
[0105] Comparative Example 1
[0106] The same as Example 2, except that the mixed conductive admixture does not contain modified conductive carbon black, and the amount of conductive carbon black used is 45 parts by mass.
[0107] Comparative Example 2
[0108] The same as Example 2, except that the mixed conductive admixture does not contain magnetic fly ash and graphite tailings.
[0109] Comparative Example 3
[0110] The same as Example 2, except that the mixed conductive admixture is replaced with graphite tailings of equal mass.
[0111] The curing methods of Examples 2 to 3 and Comparative Examples 1 to 3 are the same as those of Example 1, and all of them are powered on.
[0112] The compressive strength and slump data of different concretes are shown in Table 8.
[0113] Table 8 Compressive strength and slump of concrete
[0114]
[0115] The resistivity data of different concretes are shown in Table 9.
[0116] Table 9 Resistivity of concrete
[0117]
[0118]
[0119] It can be seen from Tables 8 and 9 that adding modified conductive carbon black to concrete can solve the problem of decreased mechanical properties of concrete caused by excessive addition of conductive carbon black, and can further improve the mechanical properties of concrete and reduce the resistivity of concrete.
[0120] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A mixed conductive admixture, characterized in that: The invention comprises the following raw materials in parts by weight: 15 to 25 parts of conductive carbon black, 25 to 39 parts of magnetic fly ash, 15 to 26 parts of crude steel slag, 5 to 15 parts of stainless steel fiber, 15 to 25 parts of graphite tailings and 30 to 40 parts of modified conductive carbon black; The preparation method of the modified conductive carbon black comprises the following steps: Conductive carbon black is ultrasonically dispersed in water, then ozone is introduced and stirred for reaction to obtain oxidized carbon black; The aramid fiber is soaked in a sulfuric acid solution and then soaked in a sodium bicarbonate solution to obtain a pretreated aramid fiber; The pretreated aramid fiber is added into a mixed solution of oxalyl chloride and dichloromethane, and heated to react to obtain chlorinated aramid fiber; Adding oxidized carbon black and chlorinated aramid fiber into an organic solvent, heating and refluxing to obtain the modified conductive carbon black; The mass ratio of the conductive carbon black to water is 1:10; the flow rate of the ozone is 60-80 mL / min; the stirring reaction time is 15-20 h; The concentration of the sulfuric acid solution is 25-30wt.%; the aramid fiber is immersed in the sulfuric acid solution for 30-40 minutes; the concentration of the sodium bicarbonate solution is 0.5wt.%; the aramid fiber is immersed in the sodium bicarbonate solution for 4-5 minutes; The amount ratio of the pretreated aramid fiber, oxalyl chloride and dichloromethane is 1g:5mL:10mL; the temperature of the heating reaction is 60-65°C and the time is 10-12h; The mass ratio of the oxidized carbon black to the chlorinated aramid fiber is 5:1; and the heating reflux reaction time is 8 to 10 hours.
2. A conductive concrete pole material that is energized and does not require steaming, characterized in that: The raw materials include: 15 parts by mass of the mixed conductive admixture according to claim 1, 12 to 20 parts by mass of cement, 23 to 35 parts by mass of sand, 25 to 44 parts by mass of crushed stone, 8 to 20 parts by mass of water and a concrete admixture; The dosage of the concrete admixture is 2.1% of the mass of cement.
3. The conductive concrete pole material for electricity supply and non-steam curing according to claim 2 is characterized in that: The concrete admixture consists of hydroxyethyl cellulose, polycarboxylate high-efficiency water reducing agent, organosilicon defoaming agent and calcium formate early strength agent in a mass ratio of 0.4:1:0.2:0.
5.
4. A method for preparing the energized steam-free conductive concrete pole material according to any one of claims 2 to 3, characterized in that: The following steps are involved: The stainless steel fiber, the concrete admixture and 1 / 2 water are mixed and stirred evenly to obtain a mixture 1; Adding sand, gravel and crude steel slag to mixture 1 and stirring evenly to obtain mixture 2; Adding graphite tailings, magnetic fly ash and cement to mixture 2, adding the remaining water after mixing evenly, stirring evenly, to obtain mixture 3; Other raw materials are added to the mixture 3 and stirred evenly to obtain the electrification-free steam-curing conductive concrete pole material.
5. Use of the energized, steam-curing-free conductive concrete pole material according to any one of claims 2 to 3 in power supply.
Citation Information
Patent Citations
Aramid fiber surface modification method
CN105002719A
Wear-resistant and compression-resistant high-performance rubber and preparation method thereof
CN110845775A
Natural grounding electric conduction concrete foundation of power transmission tower
CN116535126A
Conductive carbon black surface modification method and application
CN117343400A