A coke oven repair material and preparation method thereof
By using raw materials such as magnesium aluminum spinel powder, coke oven repair materials prepared by using raw materials such as magnesium aluminum spinel powder, the problem of insufficient thermal shock resistance and mechanical properties of existing materials is solved, and the efficient stability and corrosion resistance of coke oven repair materials are achieved, which is suitable for coking The furnace's long-term operating environment.
Patent Information
- Application Number
- CN202410182127.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-19
AI Technical Summary
The thermal shock resistance and mechanical properties of existing coke oven repair materials are poor, which leads to the easy fall off of the repair area, affecting the continuity of coking production.
Magnesium aluminum spinel powder, mullite powder, iron ore powder, aluminum powder, nickel powder, carbide, nitride, phosphorus-containing polysilazane, benzoxazine resin, lignin-modified furan resin and epoxy resin The coke oven repair materials prepared by other raw materials can improve the density and bonding strength of the material through ball milling and mixing, promote resin decomposition and carbon nanotube growth, and enhance thermal shock resistance.
It significantly improves the mechanical properties and thermal shock resistance of coke oven repair materials, ensures the stability and corrosion resistance of the repair materials at high temperatures, and is suitable for long-term operating environments of coke ovens.
Smart Images

Figure CN118307318B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of refractory materials, in particular to a coke oven repair material and a preparation method thereof. Background Art
[0002] After a long period of operation, the coking oven is often in poor condition, with holes and erosion on the furnace wall. It is necessary to continuously carry out excavation, repair and patching to ensure the integrity of the coking oven body and the stability of operation, and create conditions for the continuity of coking production and normal use.
[0003] The repair materials currently used are mostly clay mortars, which have poor thermal shock resistance and low mechanical properties, causing the repaired parts to fall off after a period of time, thus destroying the continuity of production. Summary of the invention
[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a coke oven repair material and a preparation method thereof.
[0005] The technical solutions adopted are as follows:
[0006] A coke oven repair material is prepared from the following raw materials in parts by weight:
[0007] 40-60 parts of magnesium aluminum spinel powder, 20-40 parts of mullite powder, 10-20 parts of iron ore powder, 1-3 parts of aluminum powder, 0.5-1.5 parts of nickel powder, 5-15 parts of non-metallic carbide, 5-15 parts of non-metallic nitride, 1-2 parts of phosphorus-containing polysilazane, 5-10 parts of benzoxazine resin, 3-6 parts of lignin-modified furan resin, and 5-10 parts of epoxy resin.
[0008] Furthermore, the non-metallic carbide is boron carbide.
[0009] Furthermore, the non-metallic nitride is silicon nitride and / or boron nitride.
[0010] Furthermore, the phosphorus-containing polysilazane is obtained by copolymerizing vinyl polysilazane with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0011] Furthermore, the preparation method of the phosphorus-containing polysilazane is as follows:
[0012] Under nitrogen protection, vinyl polysilazane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene are mixed, and then a free radical initiator is added. The temperature is raised to reflux for reaction for 10-24 hours. After the reaction is completed, toluene is removed by reduced pressure distillation and then vacuum drying is performed.
[0013] Furthermore, the weight ratio of vinyl polysilazane to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1:0.1-0.5.
[0014] Furthermore, the free radical initiator is any one or more combinations of cyclohexanone peroxide, dibenzoyl peroxide, tert-butyl hydroperoxide, azobisisobutyronitrile, and azobisisoheptanenitrile.
[0015] Furthermore, the amount of the free radical initiator is 0.1-1% of the total weight of vinyl polysilazane and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
[0016] Furthermore, the preparation method of the lignin-modified furan resin is as follows:
[0017] Mix formaldehyde and lignin, add urea and furfuryl alcohol, adjust the pH to 9-10, heat to 80-90℃, react for 60-90min, then add furfuryl alcohol, adjust the pH to 4-5, react for 60-120min, vacuum dehydrate after the reaction, add urea and furfuryl alcohol again, react for 1-5h, and cool to room temperature.
[0018] The present invention also provides a method for preparing a coke oven repair material:
[0019] Magnesium aluminum spinel powder, mullite powder, iron ore powder, aluminum powder, nickel powder, non-metallic carbide and non-metallic nitride are mixed and ball-milled, and then dried to obtain a mixed powder, and the mixed powder is mixed with phosphorus-containing polysilazane, benzoxazine resin, lignin-modified furan resin and epoxy resin.
[0020] Beneficial effects of the present invention:
[0021] The invention provides a coke oven repair material. Magnesium aluminum spinel has good corrosion resistance to both acidic and alkaline slags, and has a low thermal expansion coefficient and strong thermal shock resistance. Therefore, it is used as a matrix material. Mullite has good volume stability at high temperature, high mechanical strength, and resistance to high temperature creep. Iron oxide and aluminum oxide in iron ore powder can fully dissolve with magnesium aluminum spinel at high temperature to form a second bonding phase and produce a certain volume effect, fill the pores formed by carbonization and shrinkage of the resin bonding phase, and improve the density and mechanical strength of the material. The introduction of aluminum powder can effectively enhance the wetting and bonding performance between pyrolytic carbon particles generated after the resin bonding phase is decomposed by heat and other components. It is oxidized or carbonized while filling the pores, further filling the pores and improving the mechanical properties. Nickel powder can promote the decomposition of resin and the in-situ growth of carbon nanotubes. Non-metallic carbides and non-metallic nitrides have excellent high temperature properties such as high high temperature strength, good wear resistance and corrosion resistance, and can produce a "pinning" effect to limit the occurrence of slip, cavities and creep, and improve the thermal shock resistance and mechanical strength of the repair material.
[0022] Phosphorus-containing polysilazane can increase the residual carbon rate of the resin bonding phase, and as a precursor, it reacts with pyrolytic carbon to generate silicon carbide whiskers, thereby improving the mechanical properties of the material. The combination of benzoxazine resin, lignin-modified furan resin, and epoxy resin has a high residual carbon rate while ensuring the fluidity of the repair material, thereby forming more metal carbides at high temperatures. The lignin-modified furan resin has a high density of network structure formed after curing due to the introduction of more aromatic structures, which can effectively improve the bonding strength of the resin after curing and a higher residual carbon rate, thereby improving the mechanical properties of the material.
[0023] After testing, it is shown that the repair material prepared by the present invention has higher mechanical properties and thermal shock resistance, and is suitable for repairing coke ovens. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a cross-sectional SEM image of the sample prepared in Example 1 in the performance test of the present invention. DETAILED DESCRIPTION
[0025] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0026] Magnesium aluminum spinel powder: TAIMEI Japan Daming Chemical
[0027] Mullite powder: Shijiazhuang Yitian Mineral Products Co., Ltd.
[0028] Iron ore powder: Hebei Houkang Mineral Products Co., Ltd.;
[0029] Aluminum powder: Xinji Guangyuan Metal Powder Co., Ltd.
[0030] Nickel powder: Xinji Guangyuan Metal Powder Co., Ltd.
[0031] Boron carbide: Hebei Teng Bimetallic Materials Co., Ltd.;
[0032] Silicon nitride: Hebei Teng Bimetallic Materials Co., Ltd.;
[0033] Phosphorus-containing polysilazane: homemade;
[0034] Benzoxazine resin: Dongguan Xiangteng Plastic Co., Ltd.;
[0035] Lignin modified furan resin: homemade;
[0036] Epoxy resin E-51: Hebei Jingxin New Materials Co., Ltd.
[0037] Embodiment 1:
[0038] A coke oven repair material is prepared from the following raw materials in parts by weight:
[0039] 50 parts of magnesium aluminum spinel powder, 30 parts of mullite powder, 15 parts of iron ore powder, 2 parts of aluminum powder, 1 part of nickel powder, 10 parts of boron carbide, 10 parts of silicon nitride, 1.5 parts of phosphorus-containing polysilazane, 8 parts of benzoxazine resin, 5 parts of lignin-modified furan resin, and 10 parts of epoxy resin E-51.
[0040] Wherein, the preparation method of phosphorus-containing polysilazane is as follows:
[0041] Under nitrogen protection, 20g of vinyl polysilazane, 6.48g of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and 200ml of toluene were mixed, and then 0.5g of free radical initiator azobisisobutyronitrile was added. The temperature was raised to reflux for reaction for 24h. After the reaction was completed, toluene was removed by reduced pressure distillation and then vacuum dried.
[0042] The preparation method of lignin modified furan resin is as follows:
[0043] Mix 21.1g formaldehyde (37%) and 2.9g lignin, add 4.8g urea and 30g furfuryl alcohol, adjust the pH of the reaction system to 9 with 0.01mol / L sodium hydroxide solution, heat to 85°C, react for 90min, add 40g furfuryl alcohol, adjust the pH of the reaction system to 4 with 0.01mol / L hydrochloric acid solution, react for 90min, vacuum dehydrate after the reaction, add 1.2g urea and 22.5g furfuryl alcohol, react for 2.5h, and cool to room temperature.
[0044] Preparation method of the above coke oven repair material:
[0045] Magnesium aluminum spinel powder, mullite powder, iron ore powder, aluminum powder, nickel powder, boron carbide and silicon nitride are added to a planetary ball mill, mixed and ball-milled for 10 hours, and then dried to obtain a mixed powder, and then the mixed powder is mixed with phosphorus-containing polysilazane, benzoxazine resin, lignin-modified furan resin and epoxy resin.
[0046] Embodiment 2:
[0047] A coke oven repair material is prepared from the following raw materials in parts by weight:
[0048] 60 parts of magnesium aluminum spinel powder, 40 parts of mullite powder, 20 parts of iron ore powder, 3 parts of aluminum powder, 1.5 parts of nickel powder, 15 parts of boron carbide, 15 parts of silicon nitride, 2 parts of phosphorus-containing polysilazane, 10 parts of benzoxazine resin, 6 parts of lignin-modified furan resin, and 10 parts of epoxy resin E-51.
[0049] Wherein, the preparation method of phosphorus-containing polysilazane and lignin-modified furan resin is the same as that of Example 1.
[0050] Preparation method of the above coke oven repair material:
[0051] Magnesium aluminum spinel powder, mullite powder, iron ore powder, aluminum powder, nickel powder, boron carbide and silicon nitride are added to a planetary ball mill, mixed and ball-milled for 10 hours, and then dried to obtain a mixed powder, and then the mixed powder is mixed with phosphorus-containing polysilazane, benzoxazine resin, lignin-modified furan resin and epoxy resin.
[0052] Embodiment 3:
[0053] A coke oven repair material is prepared from the following raw materials in parts by weight:
[0054] 40 parts of magnesium aluminum spinel powder, 20 parts of mullite powder, 10 parts of iron ore powder, 1 part of aluminum powder, 0.5 parts of nickel powder, 5 parts of boron carbide, 5 parts of silicon nitride, 1 part of phosphorus-containing polysilazane, 5 parts of benzoxazine resin, 3 parts of lignin-modified furan resin, and 10 parts of epoxy resin E-51.
[0055] Wherein, the preparation method of phosphorus-containing polysilazane and lignin-modified furan resin is the same as that of Example 1.
[0056] Preparation method of the above coke oven repair material:
[0057] Magnesium aluminum spinel powder, mullite powder, iron ore powder, aluminum powder, nickel powder, boron carbide and silicon nitride are added to a planetary ball mill, mixed and ball-milled for 10 hours, and then dried to obtain a mixed powder, and then the mixed powder is mixed with phosphorus-containing polysilazane, benzoxazine resin, lignin-modified furan resin and epoxy resin.
[0058] Comparative Example 1:
[0059] The method is basically the same as Example 1, except that no iron ore powder is added.
[0060] Comparative Example 2:
[0061] The method is basically the same as Example 1, except that no aluminum powder is added.
[0062] Comparative Example 3:
[0063] The method is basically the same as Example 1, except that nickel powder is not added.
[0064] Comparative Example 4:
[0065] It is basically the same as Example 1, except that no boron carbide is added.
[0066] Comparative Example 5:
[0067] It is basically the same as Example 1, except that silicon nitride is not added.
[0068] Comparative Example 6:
[0069] The process is basically the same as Example 1, except that phosphorus-containing polysilazane is not added.
[0070] Comparative Example 7:
[0071] The method is basically the same as Example 1, except that the lignin-modified furan resin is not added.
[0072] Comparative Example 8:
[0073] The method is basically the same as Example 1, except that commercially available furan resin is used instead of lignin-modified furan resin.
[0074] Performance Test:
[0075] The repair materials prepared in Examples 1-3 of the present invention and Comparative Examples 1-8 were respectively injected into a mold, and after being cured at room temperature for 24 hours, demolded, dried at 130° C. for 12 hours, and heat treated at 1400° C. in an air atmosphere for 12 hours, a sample with a size of 40 mm×40 mm×160 mm was obtained. The high temperature flexural strength of the sample at 1400° C. was tested using GB / T 3002-2017;
[0076] The thermal shock resistance of the sample was determined by the rapid cooling method. The specific method was: under carbon burial conditions, the sample was kept at 1400°C for 0.5h, quickly taken out and rapidly cooled in water at room temperature for 5min, the sample was taken out and dried and the previous operation was repeated 10 times, and then the high-temperature flexural strength of the sample was tested using GB / T3002-2017. The high-temperature flexural strength decrease rate was calculated as an indicator for evaluating thermal shock resistance.
[0077] The test results are shown in Table 1 below:
[0078] Table 1:
[0079]
[0080] It can be seen from Table 1 above that the repair material prepared by the present invention has higher mechanical properties and thermal shock resistance.
[0081] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A coke oven repair material, It is characterized in that It is prepared from the following raw materials in parts by weight: 40-60 parts of magnesium aluminum spinel powder, 20-40 parts of mullite powder, 10-20 parts of iron ore powder, 1-3 parts of aluminum powder, 0.5-1.5 parts of nickel powder, 5-15 parts of non-metallic carbide, 5-15 parts of non-metallic nitride, 1-2 parts of phosphorus-containing polysilazane, 5-10 parts of benzoxazine resin, 3-6 parts of lignin-modified furan resin, and 5-10 parts of epoxy resin.
2. The coke oven repair material according to claim 1, It is characterized in that The non-metal carbide is boron carbide.
3. The coke oven repair material according to claim 1, It is characterized in that The non-metal nitride is silicon nitride and / or boron nitride.
4. The coke oven repair material according to claim 1, It is characterized in that The phosphorus-containing polysilazane is obtained by copolymerizing vinyl polysilazane and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
5. The coke oven repair material according to claim 4, It is characterized in that The preparation method of the phosphorus-containing polysilazane is as follows: Under nitrogen protection, vinyl polysilazane, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and toluene are mixed, and then a free radical initiator is added. The temperature is raised to reflux for reaction for 10-24 hours. After the reaction is completed, toluene is removed by reduced pressure distillation and then vacuum drying is performed.
6. The coke oven repair material according to claim 5, It is characterized in that The weight ratio of vinyl polysilazane to 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide is 1:0.1-0.
5.
7. The coke oven repair material according to claim 5, It is characterized in that The free radical initiator is any one or more combinations of cyclohexanone peroxide, dibenzoyl peroxide, tert-butyl hydroperoxide, azobisisobutyronitrile, and azobisisoheptanenitrile.
8. The coke oven repair material according to claim 5, It is characterized in that The amount of the free radical initiator used is 0.1-1% of the total weight of vinyl polysilazane and 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide.
9. The coke oven repair material according to claim 1, It is characterized in that The preparation method of the lignin modified furan resin is as follows: Mix formaldehyde and lignin, add urea and furfuryl alcohol, adjust the pH to 9-10, heat to 80-90℃, react for 60-90min, then add furfuryl alcohol, adjust the pH to 4-5, react for 60-120min, vacuum dehydrate after the reaction, add urea and furfuryl alcohol again, react for 1-5h, and cool to room temperature.
10. A method for preparing a coke oven repair material according to any one of claims 1 to 9, It is characterized in that Magnesium aluminum spinel powder, mullite powder, iron ore powder, aluminum powder, nickel powder, non-metallic carbide and non-metallic nitride are mixed and ball-milled, and then dried to obtain a mixed powder, and the mixed powder is mixed with phosphorus-containing polysilazane, benzoxazine resin, lignin-modified furan resin and epoxy resin.