A high swelling adhesive tape and its preparation method and application
Through the combination of porous substrate and patterned pressure-sensitive adhesive layer, the problems of easy cracking of tape at the corners of lithium-ion batteries and insufficient lithium-ion permeability are solved, and low dissolution rate, moderate swelling rate and high lithium-ion permeability are achieved. , improves battery performance and safety.
Patent Information
- Application Number
- CN202410483183.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-22
AI Technical Summary
Existing lithium-ion battery tapes are prone to cracking at corners, resulting in battery performance and safety issues, and cannot guarantee the permeability and moderate swelling of lithium ions, affecting battery density and service life.
Using a combination of porous substrate and patterned pressure-sensitive adhesive layer, the tape has low dissolution rate, moderate swelling rate and high lithium ion permeability in the electrolyte, providing mechanical properties and peeling strength.
Effectively prevent pole plates from cracking at the corners of the battery, improve battery pass rate, ensure the transmission channel of lithium ions, extend the battery life and improve safety performance.
Smart Images

Figure CN118308039B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery tapes, and in particular relates to a high swelling tape and a preparation method and application thereof. Background Art
[0002] In the normal production process of lithium batteries, the positive electrode sheets are wound with the separator and the negative electrode sheets, and then undergo processes such as hot pressing, liquid injection, and chemical formation to prepare the battery cells. Since the electrode sheets are somewhat brittle, the bending amplitude of the electrode sheets wound in the inner layer of the battery cells is often large at the corners of the battery cells, and there is a large stress, which leads to easy cracking after hot pressing, and the active material falls off, thus affecting the yield rate and safety of the battery cells, or causing lithium deposition at the corners during the battery cycle, and causing the wound battery cells to deform, so that the electrode sheets at the corners are at risk of breaking, affecting the safety performance and cycle performance of the battery.
[0003] In the field of battery tape technology, most tapes are used to fill the gap between the battery cell and the shell. When a lithium-ion battery with a metal shell is assembled, there will be a certain gap between the battery cell and the shell. If the battery cell cannot be effectively fixed in the shell, the battery cell will move in the shell after vibration or external impact, which may increase the internal resistance of the battery or damage the electrode sheet, thereby greatly deteriorating the performance of the battery. In order to effectively solve the above problems, battery tapes with high swelling rates are mostly used. After being soaked in liquid, the volume expands by swelling to fill the gap between the battery cell and the shell and fix the battery cell. However, if the above tape is used inside the battery, the battery energy density will decrease due to the excessively high swelling rate, and the tape cannot guarantee the permeability of lithium ions.
[0004] To solve the above problems, technicians in this field are looking for a tape that can be used at the corners inside the battery to provide certain mechanical properties for the corners of the battery. At the same time, since the tape is set inside the electrode, it is first necessary to ensure that it has lithium ion permeability and cannot occupy a large volume to affect the battery density. Secondly, it is not easy to fall off in an electrolyte environment.
[0005] There is a dissolving tape in the prior art. Although this tape can provide certain mechanical properties for the battery corners during hot pressing to prevent the corners from cracking and deforming during the hot pressing process, after the tape dissolves, stress still exists in the battery corners, which makes the electrode at the corner at risk of breaking, and cannot completely solve the above problem.
[0006] In order to overcome the above technical problems, the battery tape is applied to the inside of the battery corner. It is now necessary to optimize and improve the battery tape from two angles. First, the swelling rate of the substrate or the adhesive layer is controlled to ensure that it occupies a small volume while providing certain mechanical properties after swelling; second, the overall ion permeability of the tape and the peeling strength of the adhesive layer after soaking in liquid are guaranteed.
[0007] In order to solve the above problems, invention CN 114402467 A discloses a coated separator for lithium ion batteries, which contains a porous separator substrate and a coating on at least one side of the separator. The organic coating contains a silane-functionalized fluoropolymer-acrylic composition or a mixture of a silane-functionalized fluoropolymer and a non-silane-functionalized fluoropolymer. Although the separator prepared by the invention ensures the permeability of lithium ions, the addition of functional groups to the fluoropolymer to ensure the dry adhesion of the separator often softens the fluoropolymer, making it less fragile and increasing the swelling rate. However, when swollen by electrolyte, it may be too soft and lose its cohesive strength, and will not form good wet adhesion, that is, the peeling strength after soaking is low, and it may fall off during operation.
[0008] Invention CN117683218A discloses a swelling tape matrix material, swelling tape and lithium battery, the swelling tape matrix material includes a heat-resistant segment and a swelling segment, the heat-resistant segment includes polyethylene terephthalate, the swelling segment includes a linear diacid glycol ester, and the molar ratio of the heat-resistant segment to the swelling segment is (1-4): 1. The invention adds a heat-resistant segment and a swelling segment to the matrix, so that the matrix has excellent swelling, electrolysis resistance and certain mechanical strength in the electrolyte, but the tape substrate does not take into account the permeability of lithium ions, and its substrate cannot be applied between the electrode and the diaphragm. At the same time, due to its excellent swelling, after the electrolyte is adsorbed, the tape matrix volume occupies a large internal space of the battery, resulting in a decrease in battery density and thus a decrease in battery performance.
[0009] Therefore, how to provide a tape that can be used inside lithium-ion batteries, has a low dissolution rate and a moderate swelling rate, does not affect the passage of lithium ions, and still has certain mechanical properties and peel strength after being soaked in electrolyte is an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0010] In view of the defects existing in the above-mentioned prior art, the present invention provides a high swelling type adhesive tape and a preparation method and application thereof. The high swelling type adhesive tape is particularly suitable for the interior of lithium ion batteries and has comprehensive properties such as low dissolution rate, moderate swelling rate, good lithium ion permeability and stable mechanical properties.
[0011] In a first aspect, the present invention provides a high swelling adhesive tape, comprising a porous substrate and a pressure-sensitive adhesive layer;
[0012] The porous substrate has a thickness of 5-50 μm and is selected from at least one of a porous polymer membrane and a non-woven fabric;
[0013] The thickness of the pressure-sensitive adhesive layer is 0.5-50 μm, and the area covered by the porous substrate accounts for 10-50% of the total area of the porous substrate;
[0014] The pressure-sensitive adhesive layer comprises at least one of the raw materials of composition (1) and composition (2):
[0015] Composition (1) includes: a rubber component, a viscosity modifier and a tackifying resin;
[0016] Composition (2) includes: a carboxyl / hydroxyl terminated acrylate resin and a curing agent;
[0017] The dissolution rate of the pressure-sensitive adhesive layer in the electrolyte is less than 5%, the swelling rate is greater than 100%, and the average maximum peeling force after soaking in the electrolyte is above 1N.
[0018] The present invention adopts a pressure-sensitive adhesive layer with low dissolution rate and high swelling property. During the winding process, the pressure-sensitive adhesive layer sticks the tape to the place where the pole piece is bent with a large amplitude. In the subsequent hot pressing process, it can effectively prevent the pole piece from cracking, improve the qualified rate of the battery product, and the pressure-sensitive adhesive layer can quickly absorb a large amount of electrolyte in the subsequent liquid injection process, and the volume swells, and a large number of solvent channels are formed in the adhesive layer, so as not to affect the transmission of lithium ions. In addition, during the battery cycle, the risks and problems such as lithium deposition, deformation and fracture of the battery cell corners are reduced. In addition, the pressure-sensitive adhesive layer only covers part of the porous substrate, and on the basis of ensuring sufficient bonding performance before and after the bubble, the ion permeability of the tape is further improved. In actual use, the swelling rate needs to be controlled within a certain range, for example, less than 300%, preferably less than 200%, on the basis of being greater than 100%, preferably greater than 120%. Different from the existing swelling tapes which have a particularly high swelling rate to provide a particularly large volume after the bubble to fill the gap, the tape of the present invention needs to control the swelling rate within a reasonable range, otherwise the bubble bonding performance of the tape will be destroyed.
[0019] Preferably, the pressure-sensitive adhesive layer is patterned and covers the surface of the porous substrate, and the coverage area accounts for 20-40% of the total area of the porous substrate.
[0020] Selecting the appropriate pressure-sensitive adhesive layer coverage area and the appropriate adhesive layer swelling rate can ensure sufficient ion permeability and bonding strength before and after the tape is soaked. For example, when the pressure-sensitive adhesive layer covers a large area, a pressure-sensitive adhesive layer with a higher swelling rate is required to ensure that the tape as a whole has sufficient ion permeability; when the pressure-sensitive adhesive layer covers a small area, since the porous substrate basically provides good ion permeability, the pressure-sensitive adhesive layer swelling rate can be slightly lower to provide sufficient bonding strength.
[0021] Preferably, the pattern includes at least one of a dot-shaped spaced pattern, a line-shaped spaced pattern, and a grid pattern.
[0022] The patterned adhesive layer can not only maintain physical stability after swelling to prevent the tape from breaking or deforming, but also promote the transmission of lithium ions through a variety of pattern designs, such as dot-shaped spacing patterns, linear spacing patterns (including straight lines, zebra patterns, etc.) and / or grid patterns, etc. In addition, the above two raw material compositions can be used simultaneously to form a pressure-sensitive adhesive layer with a combined pattern, such as a design of spaced dots, stripes, etc., using the swelling, adhesion and other characteristics of the two raw material compositions to form a synergistic effect on the tape as a whole. Preferably, the area ratio of the pressure-sensitive adhesive layer formed by the raw material of composition (1) and the raw material of composition (2) on the porous substrate is (1-4): (4-1).
[0023] Preferably, the porous polymer membrane is selected from at least one of a porous PP membrane, a porous PE membrane, a porous PI membrane, a porous PAN membrane, a porous PVDF membrane, and a porous PMMA membrane, and has a porosity of 30-85%;
[0024] The non-woven fabric comprises at least one of PP non-woven fabric, PE non-woven fabric, PET non-woven fabric and PTFE non-woven fabric, and the pore size is ≤10 μm.
[0025] The porous polymer diaphragm used in the present invention balances the swelling performance and the lithium ion permeability by adjusting the pore size and distribution and the structural design of the patterned glue layer, thereby ensuring that lithium ions can pass through effectively.
[0026] Preferably, in parts by mass, composition (1) comprises:
[0027] 20-50 parts of rubber component;
[0028] 5-20 parts of viscosity modifier;
[0029] 40-60 parts of tackifying resin;
[0030] The rubber component has a molecular weight of 200,000-6000,000Da and is selected from at least one of SIS rubber, SEBS rubber, SEPS rubber and SBR rubber;
[0031] The viscosity modifier is selected from at least one of liquid polyolefin and naphthenic mineral oil;
[0032] The tackifying resin is selected from at least one of (hydrogenated) C5 petroleum resin, (hydrogenated) C9 petroleum resin, C5 / C9 copolymerized petroleum resin, and (hydrogenated) DCPD resin.
[0033] Preferably, in parts by mass, composition (2) comprises:
[0034] 95-100 parts of carboxyl / hydroxyl terminated acrylate resin;
[0035] 1-5 parts of curing agent;
[0036] The molecular weight of the carboxyl / hydroxyl terminated acrylate resin is 20,000-100,000 Da;
[0037] The curing agent is selected from at least one of multifunctional epoxy and multifunctional isocyanate.
[0038] Preferably, the pressure-sensitive adhesive layer further comprises: a filler having a particle size of 1 nm-25 μm, the amount of the filler accounting for 10-30% of the total weight of the remaining components of the pressure-sensitive adhesive layer; and / or
[0039] The carbonate compound is used in an amount of 1-3% of the total weight of the other components of the pressure-sensitive adhesive layer, and is selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, and methyl propyl carbonate. Adding a small amount of filler and / or carbonate compound is beneficial to quickly increase the swelling channel of the adhesive layer and regulate the swelling rate / time of the pressure-sensitive adhesive layer.
[0040] In a second aspect, the present invention further provides a method for preparing a high swelling adhesive tape, comprising the following steps:
[0041] Step 1: Prepare the pressure-sensitive adhesive coating liquid:
[0042] Weigh each component according to the raw material composition, and mix each component with the solvent to obtain a coating liquid;
[0043] Step 2: Coating and film forming:
[0044] The coating liquid is coated on a porous substrate and dried to form a pressure-sensitive adhesive layer to obtain a high swelling adhesive tape; or
[0045] The coating liquid is first coated on a release film, and after drying, is transferred to a porous substrate to form a pressure-sensitive adhesive layer, thereby obtaining a high-swelling adhesive tape.
[0046] Optionally, a release layer may be formed on the tape to facilitate winding, and accordingly, step 3 may be added after step 2. For example, step 3, tape winding: a release agent is applied on the back of the porous substrate or a release film is provided on the surface of the pressure-sensitive adhesive layer, and the tape is wound to form a single-sided high-swelling tape.
[0047] Preferably, the solvent in step 1 is an organic solvent, including at least one of toluene, xylene, methylcyclohexane, ethyl acetate, butyl acetate, butanone, methyl isobutyl ketone, ethanol, and isopropanol, and the solid content of the coating liquid is 5-60%. The above solvent can form a substantially uniform coating liquid from the raw material components.
[0048] In a third aspect, the present invention also provides an application of the high swelling type adhesive tape in protecting lithium battery pole pieces, pole tabs, and winding and finishing.
[0049] The present invention has at least the following beneficial effects:
[0050] (1) The present invention prepares an adhesive tape by using a porous polymer substrate and a discontinuously distributed pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer can not only maintain physical stability after swelling to prevent the tape from breaking or deforming, but also adjust the area ratio of the porous polymer substrate covered by a specific pattern design to promote the transmission of lithium ions. The swelling ability of the tape needs to be optimized through the chemical composition and structural design of the pressure-sensitive adhesive layer to ensure sufficient electrolyte absorption to achieve the swelling effect. At the same time, the present invention adjusts the pore size and distribution of the substrate, as well as the structure of the patterned adhesive layer, which together ensure that lithium ions can pass effectively.
[0051] (2) The present invention adopts carboxyl / hydroxyl terminated acrylate resin as the main component of the adhesive layer, which not only ensures good bonding performance between the substrate and the electrode, but also has excellent corrosion resistance and thermal stability. The introduction of carboxyl and hydroxyl groups helps to enhance the mutual solubility between the resin and the electrolyte, promotes the absorption and retention of the electrolyte, and can make the swollen tape have better lithium ion permeability, because more electrolyte can be stored in the pressure-sensitive adhesive layer of the tape, providing sufficient medium for lithium ion transmission.
[0052] (3) Carboxyl / hydroxyl terminated acrylate resin can improve the mechanical strength and flexibility of the adhesive layer. It can effectively prevent the adhesive tape from breaking or being damaged due to volume changes during the battery charging and discharging process, thereby improving the reliability and service life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] Figure 1 It is a schematic diagram of the structure of the high swelling type adhesive tape of the present invention.
[0054] Reference numerals: 1 - pressure-sensitive adhesive layer, 2 - porous substrate. DETAILED DESCRIPTION
[0055] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0056] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "said" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings, and "multiple" generally includes at least two.
[0057] It should also be noted that the term "includes", "comprising" or any other variation thereof is intended to cover non-exclusive inclusion, so that a commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprising a ..." do not exclude the existence of other identical elements in the commodity or device including the elements.
[0058] Participate in the Figure 1 The high swelling adhesive tape of the present invention comprises a porous substrate 2 and a pressure-sensitive adhesive layer 1, wherein:
[0059] 1. The porous substrate 2 is selected from at least one porous polymer membrane selected from porous PP film, porous PE film, porous PI film, porous PAN film, porous PVDF film, porous PMMA film with a porosity of 30-85% or at least one non-woven fabric selected from PP non-woven fabric, PE non-woven fabric, PET non-woven fabric, PTFE non-woven fabric with a pore size of ≤10μm.
[0060] 2. The pressure-sensitive adhesive layer 1 comprises at least one of the raw materials of component (1) and component (2); optionally, a filler having a particle size of 1 nm-25 μm, the amount of which accounts for 10-30% of the total weight of the other components of the pressure-sensitive adhesive layer 1, the filler including but not limited to at least one of boehmite, talc, and silica, the filler may be porous or non-porous, and may be compounded with different particle sizes; and / or its amount accounts for 1-3% of the total weight of the other components of the pressure-sensitive adhesive layer 1, and is composed of at least one carbonate compound selected from ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, and methylpropyl carbonate, wherein:
[0061] Composition (1) is calculated by weight and comprises:
[0062] 20-50 parts of rubber component;
[0063] 5-20 parts of viscosity modifier;
[0064] 40-60 parts of tackifying resin;
[0065] The rubber component has a molecular weight of 200,000-6000,000Da and is selected from at least one of SIS rubber, SEBS rubber, SEPS rubber, and SBR rubber; the viscosity modifier is selected from at least one of liquid polyolefins and cycloalkyl mineral oils; the tackifying resin is selected from at least one of (hydrogenated) C5 petroleum resin, (hydrogenated) C9 petroleum resin, C5 / C9 copolymerized petroleum resin, and (hydrogenated) DCPD resin.
[0066] Composition (2) is calculated by weight and comprises:
[0067] 95-100 parts of carboxyl / hydroxyl terminated acrylate resin;
[0068] 1-5 parts of curing agent;
[0069] The molecular weight of the carboxyl / hydroxyl terminated acrylate resin is 20,000-100,000 Da;
[0070] The curing agent is selected from at least one of multifunctional epoxy and multifunctional isocyanate.
[0071] The area of the porous substrate 2 covered by the pressure-sensitive adhesive layer 1 accounts for 10-50% of the total area of the porous substrate 2. Preferably, the pressure-sensitive adhesive layer 1 is patterned and covers the surface of the porous substrate 2, and the coverage area accounts for 20-40% of the total area of the porous substrate 2. Specifically, the pattern includes at least one of a dot-like spacing pattern, a line-like spacing pattern, and a grid pattern.
[0072] In addition, the present invention can also pattern-coat the surface of the porous substrate 2 according to the raw material composition of composition (1) and composition (2), respectively, to give full play to their respective advantages, and jointly obtain a composite adhesive tape with designable swelling rate and adhesive performance. The area ratio of the pressure-sensitive adhesive layer 1 formed by the raw material of composition (1) and the raw material of composition (2) on the porous substrate 2 is (1-4): (4-1).
[0073] The carboxyl / hydroxyl terminated acrylate resin can be prepared by a thermal initiation method or a photoinitiation method.
[0074] The thermal initiation method for preparing hydroxyl / carboxyl terminated acrylic resin comprises:
[0075] I) heating the reactor to 40-50° C., adding 3-6 parts of acrylate prepolymer, 80-120 parts of common acrylate monomer, and 140-160 parts of solvent by weight, and stirring at 30-60 rpm for 30-90 min;
[0076] II) heating to 55-65° C. and passing nitrogen, then dropwise adding a portion (about 5-8 parts, accounting for 50-65% of the total solution) of a thermal initiator solution (solid content 0.5-1.5 wt%) and 140-150 parts of a solvent, and stirring at 20-60 rpm for at least 4 hours;
[0077] III) When the viscosity reaches 9,000±200cps and the molecular weight reaches 12,000±300Da, add another portion (about 2-4 portions, accounting for 25-35% of the total solution) of thermal initiator solution and
[0078] 140-155 parts of solvent, raise the temperature to 70-75°C and continue the reaction for at least 3 hours;
[0079] IV) When the viscosity and molecular weight meet the requirements (for example, the viscosity reaches 14,000 ±
[0080] 200cps, molecular weight reaches 40,000±300Da), add the remaining thermal initiator solution (about 0.5-1.5 parts, accounting for 10-15% of the total solution), 145-155 parts of solvent and 1-3 parts of end-capping acrylate monomer, and react for 3-5 hours;
[0081] V) Discharge the material when the viscosity and molecular weight reach the requirements (for example, the viscosity reaches 20,000±200cps, and the molecular weight reaches 50,000±300Da).
[0082] The photoinitiator method is used to prepare a hydroxyl / carboxyl terminated acrylic resin, comprising:
[0083] I) adding 3-6 parts of acrylate prepolymer, 80-120 parts of common acrylate monomer and 140-160 parts of solvent into a reaction kettle, and stirring at a speed of 30-60 rpm for 30-90 min;
[0084] II) nitrogen is passed through, and then a portion (about 4-6 parts, accounting for 45-55% of the total solution) of photoinitiator solution (solid content 0.5-1.5wt%) and 140-150 parts of solvent are added, and stirred at 20-40rpm for at least 30min;
[0085] III) Use ultraviolet light (e.g. LED 365nm wavelength) to irradiate the side wall of the reactor at a distance of 10±1cm and a power of 5-15mW / cm 2 When the viscosity reaches 9,000±200cps and the molecular weight reaches 12,000±300Da, add another portion (about 3-5 parts, accounting for 35-45% of the total solution) of photoinitiator solution (140-150 parts of solvent) and increase the speed to 55-65rpm;
[0086] IV) when the viscosity and molecular weight reach the requirements (e.g., the viscosity reaches 14,000±200cps, and the molecular weight reaches 40,000±300Da), add the remaining photoinitiator solution (about 0.5-1.5 parts, accounting for 10-20% of the total solution), 145-155 parts of solvent, and 1-3 parts of end-capping acrylate monomer;
[0087] V) When the viscosity and molecular weight reach the required values (for example, the viscosity reaches 20,000±200 cps, and the molecular weight reaches 50,000±300 Da), stop irradiation and discharge the material.
[0088] Among them, the acrylate prepolymer is preferably a bifunctional acrylate prepolymer: epoxy-modified polyurethane, polyether polyurethane, polyester polyurethane and polycarbonate polyurethane acrylate resin, etc., with a molecular weight of 2,000-6,000Da;
[0089] Photoinitiator: 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 1-hydroxycyclohexyl phenyl ketone, α,α-dimethoxy-α-phenylacetophenone, 2,4-dihydroxybenzophenone, etc. The amount of photoinitiator added is 0.1%-0.5% of the total mass of the prepolymer and the monomer.
[0090] Thermal initiator: azobisisobutylnitrile, azobisisoheptylnitrile, dimethyl azobisisobutyrate, dibenzoyl peroxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, tert-butyl perbenzoate, tert-butyl peroxyvalerate, etc. The amount of thermal initiator added is 0.1%-0.5% of the total mass of the prepolymer and the monomer.
[0091] Common acrylate monomers: tricyclodecane dimethanol diacrylate, triethylene glycol acrylate, triethylene glycol dimethacrylate, ethoxylated bisphenol A acrylate, ethoxylated bisphenol A dimethacrylate, propoxylated neopentyl glycol diacrylate.
[0092] Monomers for hydroxyl-terminated acrylic ester copolymers: one or more of hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, propyl methacrylate, hydroxybutyl acrylate, and hydroxybutyl methacrylate.
[0093] Monomer for carboxyl-terminated acrylate copolymer: at least one of acrylic acid and methacrylic acid.
[0094] Solvents: ethyl acetate, butyl acetate, toluene, methyl isobutyl ketone, butanone, etc.
[0095] A method for preparing the high swelling adhesive tape comprises the following steps:
[0096] Step 1: Prepare the coating liquid for the pressure-sensitive adhesive layer 1:
[0097] Weighing each component according to the raw material composition, and uniformly mixing each component with a solvent to obtain a coating liquid; the solvent is an organic solvent, including at least one of toluene, xylene, methylcyclohexane, ethyl acetate, butyl acetate, butanone, methyl isobutyl ketone, ethanol, and isopropanol, and the solid content of the coating liquid is 5-60wt%;
[0098] Step 2: Coating and film forming:
[0099] The coating liquid is coated on a porous substrate 2 and dried to form a pressure-sensitive adhesive layer 1 to obtain a high swelling adhesive tape; or
[0100] The coating liquid is first coated on a release film, and after drying, is transferred to a porous substrate 2 to form a pressure-sensitive adhesive layer 1, thereby obtaining a high-swelling adhesive tape.
[0101] Optional step three, tape winding: coating a release agent on the back of the porous substrate 2 or placing a release film on the surface of the pressure-sensitive adhesive layer 1, and winding the tape to produce a single-sided high-swelling tape.
[0102] In addition, according to the respective advantages of composition (1) and composition (2), composition (1) and composition (2) are respectively configured into a first coating liquid and a second coating liquid, and a first pressure-sensitive adhesive area and a second pressure-sensitive adhesive area are formed on the porous substrate 2 successively or simultaneously, thereby forming a composite tape. The adhesive properties, dissolution rate and swelling rate of the tape are regulated according to the coverage area, thickness, composition and other conditions of the coating liquid.
[0103] In the high swelling tape of the present invention, the dissolution rate of the pressure-sensitive adhesive layer 1 in the electrolyte is less than 5%, preferably less than 3%, and more preferably less than 1.7%; the swelling rate is greater than 100%, preferably greater than 120%, and less than 200%, and the average maximum peeling force after immersion in the electrolyte is above 1N.
[0104] The raw materials used in the following examples are shown in Table A, which is only used as a reference and is not intended to limit the present invention.
[0105] Table A
[0106]
[0107]
[0108] Preparation Example 1:
[0109] The preparation method of the high swelling tape sample comprises the following steps:
[0110] Step 1: Prepare the pressure-sensitive adhesive coating liquid:
[0111] Weigh each component according to the raw material ratio of composition (1), and mix each component with a solvent to obtain a coating liquid; the solvent is toluene, and the solid content of the coating liquid is 15wt%;
[0112] Step 2: Coating and film forming:
[0113] The coating liquid is first coated on a release film, and after drying, transferred to a porous PP film substrate to form a pressure-sensitive adhesive layer;
[0114] The porosity of the porous PP film substrate is 45±10%.
[0115] Preparation Example 1 corresponds to the samples of Examples 1-1 to 1-10, and the specific parameters are shown in Table 1-1:
[0116] Table 1-1
[0117]
[0118]
[0119] Preparation Example 2:
[0120] The preparation method of the high swelling tape sample comprises the following steps:
[0121] Step 1: Prepare the pressure-sensitive adhesive coating liquid:
[0122] Weigh each component according to the raw material ratio of composition (1), and mix each component with a solvent to obtain a coating liquid; the solvent is toluene, and the solid content of the coating liquid is 15wt%;
[0123] Step 2: Coating and film forming:
[0124] The coating liquid is first coated on a release film, and after drying, is transferred to a PP non-woven fabric substrate to form a pressure-sensitive adhesive layer.
[0125] Preparation Example 2 corresponds to the samples of Examples 1-11 to 1-18, and the specific parameters are shown in Table 1-2:
[0126] Table 1-2
[0127]
[0128]
[0129] Preparation Example 3:
[0130] The preparation method of the high swelling tape sample comprises the following steps:
[0131] Step 1: Prepare the pressure-sensitive adhesive coating liquid:
[0132] The components are weighed according to the raw material ratio of composition (2), and the components are uniformly mixed with a solvent to obtain a coating liquid; the solvent is ethyl acetate, and the solid content of the coating liquid is 20 wt%.
[0133] Step 2: Coating and film forming:
[0134] The coating liquid is first coated on a release film, and after drying, transferred to a porous PP film substrate to form a pressure-sensitive adhesive layer;
[0135] The porosity of the porous PP film is 45±10%.
[0136] Preparation Example 3 corresponds to the samples of Examples 2-1 to 2-9. The specific parameters are shown in Table 2-1.
[0137] Table 2-1
[0138]
[0139]
[0140] Preparation Example 4:
[0141] The preparation method of the high swelling tape sample comprises the following steps:
[0142] Step 1: Prepare the pressure-sensitive adhesive coating liquid:
[0143] Weigh each component according to the raw material ratio of composition (2), and mix each component with a solvent to obtain a coating liquid; the solvent is ethyl acetate, and the solid content of the coating liquid is 20wt%;
[0144] Step 2: Coating and film forming:
[0145] The coating liquid is first coated on a release film, and after drying, is transferred to a PP non-woven fabric substrate to form a pressure-sensitive adhesive layer.
[0146] Preparation Example 4 corresponds to the samples of Examples 2-10 to 2-17, and the specific parameters are shown in Table 2-2:
[0147] Table 2-2
[0148]
[0149] Example 3
[0150] The preparation method of the high swelling tape sample comprises the following steps:
[0151] Step 1: Prepare the pressure-sensitive adhesive coating liquid:
[0152] First coating liquid: refer to the composition of Example 1-3 (1) raw material ratio;
[0153] Second coating liquid: refer to the composition (2) of Example 2-2 for raw material ratio;
[0154] Step 2: Coating and film forming:
[0155] The first coating liquid and the second coating liquid are respectively coated on the release film, and after drying, they are transferred to a porous PP film substrate (thickness 16 μm, porosity 45±10%) to form a first pressure-sensitive adhesive area and a second pressure-sensitive adhesive area. The first pressure-sensitive adhesive area and the second pressure-sensitive adhesive area are in a dot pattern spaced apart from each other. The dot pattern has a thickness of 3±0.2 μm, a coverage area ratio of approximately 1:1, and a total coverage area ratio of 30%.
[0156] Test method:
[0157] (1) Electrolyte resistance test-swelling rate test
[0158] Test method: take out about 2g of glue that has been cured at room temperature for 24 hours and weigh it, record the weight M1, put the glue in a PP cup, add 50g of electrolyte into the PP cup (the specific composition and ratio of the electrolyte solvent are: diethyl carbonate DEC: 50%, ethylene carbonate EC: 30%, ethyl methyl carbonate EMC: 20%), cover the lid, seal it with tape, place the sealed PP cup in an oven, bake it at 85℃ for 24hrs, wipe off the glue and weigh it immediately, record the weight M2, and calculate the swelling rate by the formula = (M2-M1)×100% / M1.
[0159] (2) Electrolyte resistance test-dissolution rate test
[0160] Test method: take out about 1.4g of glue that has been cured at room temperature for 24 hours and weigh it, record the weight M1, put the glue in a vial, add 7g of electrolyte into the vial (the specific composition and ratio of the electrolyte solvent are: diethyl carbonate DEC: 50%, ethylene carbonate EC: 30%, ethyl methyl carbonate EMC: 20%), record the weight M2, cover the lid and seal it, place the sealed vial in an oven, adjust it to 85℃ and bake it for 24hrs, draw out with a syringe, drop 15-20mg into the TGA crucible, and the test program is heated from 30-320℃ at a rate of 10℃ / min. When the program ends, record the remaining weight percentage A at 300℃, and calculate the dissolution rate by the formula = A×M2×100% / M1.
[0161] (3) Peel force test method - before soaking
[0162] Test method: Clean the aluminum foil to be tested with isopropyl alcohol and dry it, cut the tape sample into strips with a width of 24mm and a length of 100mm; stick the test surface of the tape strip to the aluminum foil to be tested to avoid bubbles or wrinkles, and use a 2kg pressure wheel to slowly press three times back and forth at a speed of 300mm / min; stick the back of the aluminum foil (the side without tape) to the stainless steel plate with double-sided tape, start the timer, and maintain for 20min; fix one end of the stainless steel plate on the lower fixture of the tensile testing machine and make it perpendicular to the horizontal plane, and reset the equipment; clamp the substrate of the tape strip with another fixture, and perform a peeling test at a speed of 304.8mm / min. Select a section with stable data (not shorter than 80mm) to calculate the peeling force, in N.
[0163] (4) Peel force test method - after soaking
[0164] Test method: Clean the aluminum foil to be tested with isopropyl alcohol and dry it, cut the tape sample into strips with a width of 24mm and a length of 100mm, stick the test surface of the tape strip to the aluminum foil to be tested to avoid bubbles or wrinkles, and use a 2kg pressing wheel to slowly press back and forth three times at a speed of 300mm / min; start the timer and maintain for 20min; put in the electrolyte solvent (the specific composition and ratio of the electrolyte solvent are: diethyl carbonate DEC: 50%, ethylene carbonate EC: 30%, ethyl methyl carbonate EMC: 20%) in a container that does not cover the liquid surface, seal it and bake it at 85℃ for 24hrs, then take it out and wipe off the surface solvent; stick the back of the aluminum foil (the side without tape) to the stainless steel plate with double-sided tape, start the timer and leave it for 20min; fix one end of the stainless steel plate on the lower fixture of the tensile testing machine and make it perpendicular to the horizontal plane, and reset the equipment; clamp the substrate of the tape sample with the other fixture, and perform a peeling test at a speed of 304.8mm / min, and select a section with stable data (not shorter than 80mm) to calculate the peeling force, unit N.
[0165] The test results for the above embodiments are shown in Tables 1-3, 1-4 and 2-3, 2-4:
[0166] Table 1-3
[0167]
[0168] Table 1-4
[0169]
[0170] Table 2-3
[0171]
[0172] Table 2-4
[0173]
[0174] The test results of Example 3 are shown in Table 3-1:
[0175] Table 3-1
[0176]
[0177] The swelling rates of the samples in the embodiments of the present invention are all greater than 100%, preferably greater than 120%, and maintained at less than 200%. The dissolution rate is less than 5%, preferably less than 3%, and more preferably less than 1.7%. A tape with a low dissolution rate and a moderate swelling rate is provided. On the basis of maintaining high ion permeability, the pressure-sensitive adhesive layer has good bonding properties before and after soaking, thereby meeting the application requirements of the tape in batteries.
[0178] Compared with the composition (1) containing the rubber component, the sample of the composition (2) containing the carboxyl / hydroxyl terminated acrylate resin has higher overall swelling rate and bonding performance and lower dissolution rate. Referring to Example 3-1, the combination of the two compositions can make the comprehensive performance of the tape designable, which is conducive to expanding the scope of application.
[0179] The samples using fillers had relatively lower dissolution rates, but the bonding properties were also reduced.
[0180] Samples containing a small amount of carbonate compounds can accelerate the swelling of the pressure-sensitive adhesive layer, showing a slightly higher but allowable dissolution rate, as well as moderate swelling rate and bonding performance.
[0181] In general, the high swelling adhesive tape of the present invention has comprehensive properties such as low dissolution rate, moderate swelling rate, high ion permeability, stable bonding performance, etc., and has a wide range of structural / performance designability and broad application prospects.
[0182] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they are aware of the basic creative concepts. Therefore, the present invention is intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention. Obviously, those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention.
Claims
1. A high swelling adhesive tape, characterized in that: including a porous substrate and a pressure-sensitive adhesive layer; The porous substrate has a thickness of 5-50 μm and is selected from at least one of a porous polymer membrane and a non-woven fabric; The thickness of the pressure-sensitive adhesive layer is 0.5-50 μm, and the area covered by the porous substrate accounts for 20-50% of the total area of the porous substrate; The pressure-sensitive adhesive layer comprises at least one of the raw materials of composition (1) and composition (2): In parts by mass, composition (1) comprises: 20-50 parts of rubber component; 5-20 parts of viscosity modifier; 40-60 parts of tackifying resin; The rubber component has a molecular weight of 200,000-6000,000Da and is selected from at least one of SIS rubber, SEBS rubber, SEPS rubber and SBR rubber; The viscosity modifier is selected from at least one of liquid polyolefin and naphthenic mineral oil; The tackifying resin is selected from at least one of (hydrogenated) C5 petroleum resin, (hydrogenated) C9 petroleum resin, C5 / C9 copolymerized petroleum resin, and (hydrogenated) DCPD resin; In parts by mass, composition (2) comprises: 95-100 parts of carboxyl / hydroxyl terminated acrylate resin; 1-5 parts of curing agent; The molecular weight of the carboxyl / hydroxyl terminated acrylate resin is 20,000-100,000 Da; The curing agent is selected from at least one of multifunctional epoxy and multifunctional isocyanate; The dissolution rate of the pressure-sensitive adhesive layer in the electrolyte is less than 5%, the swelling rate is greater than 100%, and the average maximum peeling force after soaking in the electrolyte is above 1N.
2. The high swelling adhesive tape according to claim 1, characterized in that: The pressure-sensitive adhesive layer is patterned and covered on the surface of the porous substrate, and the coverage area accounts for 20-40% of the total area of the porous substrate.
3. The high swelling adhesive tape according to claim 2, characterized in that: The pattern includes at least one of a dot-shaped spaced pattern, a line-shaped spaced pattern, and a grid pattern.
4. The highly swellable adhesive tape according to any one of claims 1 to 3, characterized in that: The porous polymer membrane is selected from at least one of a porous PP membrane, a porous PE membrane, a porous PI membrane, a porous PAN membrane, a porous PVDF membrane, and a porous PMMA membrane, and has a porosity of 30-85%; The non-woven fabric comprises at least one of PP non-woven fabric, PE non-woven fabric, PET non-woven fabric and PTFE non-woven fabric, and the pore size is ≤10 μm.
5. The high swelling adhesive tape according to claim 1, characterized in that: The pressure-sensitive adhesive layer further comprises: a filler having a particle size of 1 nm-25 μm, the amount of the filler accounting for 10-30% of the total weight of the remaining components of the pressure-sensitive adhesive layer; and / or The carbonate compound is used in an amount of 1-3% of the total weight of the other components of the pressure-sensitive adhesive layer, and is selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, and methylpropyl carbonate.
6. A method for preparing the high swelling adhesive tape according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: Prepare the pressure-sensitive adhesive coating liquid: Weigh each component according to the raw material composition, and mix each component with the solvent to obtain a coating liquid; Step 2: Coating and film forming: The coating liquid is coated on a porous substrate and dried to form a pressure-sensitive adhesive layer to obtain a high swelling adhesive tape; or The coating liquid is first coated on a release film, and after drying, is transferred to a porous substrate to form a pressure-sensitive adhesive layer, thereby obtaining a high-swelling adhesive tape.
7. The preparation method according to claim 6, characterized in that: The solvent in step 1 is an organic solvent, including at least one of toluene, xylene, methylcyclohexane, ethyl acetate, butyl acetate, butanone, methyl isobutyl ketone, ethanol, and isopropanol, and the solid content of the coating liquid is 5-60wt%.
8. Use of the high swelling adhesive tape according to any one of claims 1 to 5 in lithium battery pole piece protection, pole lug protection, and winding finishing.
Citation Information
Patent Citations
Hybrid functionalized fluoropolymers for lithium ion batteries
CN114402467A
Swelling adhesive tape base material, swelling adhesive tape and lithium battery
CN117683218A
Isolating membrane for lithium ion secondary battery
CN104852008A
High-safety regular matrix coated cohesive lithium ion battery diaphragm as well as preparation method and application thereof
CN111599971A
Binder resin composition, porous seperator comprising thereof, electrochemical element using thereof
KR1020140147742A