A high-capacity thin-film tantalum electrolytic capacitor and its preparation process

By using graphite and modified nano-silver powder materials in tantalum capacitors, combined with modified nano-silver powder and Ta2O5 films, the problem of high ESR values ​​of tantalum capacitors in high-frequency circuits is solved, achieving lower ESR values ​​and higher conductivity. efficiency, improving the high-frequency performance of the capacitor.

CN118315199BActive Publication Date: 2024-10-29SHANGHAI YONGMING ELECTRONIC CO LTD
View PDF 2 Cites -1 Cited by

Patent Information

Application Number
CN202410503030.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-10-29
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing tantalum capacitors have high ESR values ​​in high-frequency circuits. In particular, the manufacturing level and extraction efficiency of the cathode MnO2 layer have the greatest impact on capacitor performance, making it difficult to meet the requirements for low ESR values ​​in cutting-edge fields.

Method used

Graphite and modified nano-silver powder are used as cathode materials. The modified nano-silver powder improves the conductivity of the polymer silver paste and reduces the ESR value of the capacitor. The specific process includes preparing modified nano-silver powder and combining it with the graphite layer and Ta2O5 film to form a high Capacity thin film tantalum electrolytic capacitors.

Benefits of technology

It effectively reduces the ESR value of the capacitor, improves the conductivity and stability, and significantly improves the high-frequency performance of the capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-capacity thin-film tantalum electrolytic capacitor and a preparation process thereof. The high-capacity thin-film tantalum electrolytic capacitor comprises an anode tantalum core, a positive electrode lead is fixedly connected at the center of one end of the anode tantalum core, the positive electrode lead is a tantalum wire, a Ta2O5 film is provided on the surface of the anode tantalum core, a manganese dioxide layer is provided on the outer layer of the Ta2O5 film, a graphite layer is provided on the outer layer of the manganese dioxide layer, a polymer silver paste layer is provided on the outer layer of the graphite layer, the polymer silver paste layer comprises the following raw materials by weight: 40-50 parts of modified nano silver powder, 5-10 parts of bisphenol A epoxy resin, 1-2 parts of curing agent, 3-5 parts of ethyl acetate, 0.5-1 parts of active diluent, the polymer silver paste layer is coated with a silver shell, and the silver shell is fixedly connected to the negative electrode lead. The invention uses graphite and polymer silver paste as cathode lead-out materials, and the polymer silver paste uses modified nano silver powder as a conductive material, and the modified nano silver powder effectively improves the conductivity of the polymer silver paste, thereby reducing the ESR value of the capacitor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tantalum capacitors, and in particular relates to a high-capacity thin-film tantalum electrolytic capacitor and a preparation process thereof. Background Art

[0002] As an indispensable passive electronic component in electronic circuits, capacitors have important applications in filtering, bypassing, coupling, etc. Among the many types of capacitors, tantalum electrolytic capacitors have excellent properties such as high reliability and low leakage current, and are widely used in cutting-edge fields such as national defense and aerospace. Solid tantalum electrolytic capacitors have excellent performance and are the smallest and largest capacitors. Tantalum electrolytic capacitors use metal tantalum blocks as anodes. The sintered anode tantalum blocks are placed in an energy-enabling tank, and a uniform oxide film, namely tantalum pentoxide, is generated on its surface as a medium. Manganese dioxide or conductive polymers decomposed from manganese nitrate solution at high temperature are used as electrolytes. Carbon and silver are used as cathodes, and the electrical energy is drawn out through leads.

[0003] With the continuous improvement of the overall performance of military electronic equipment with reliability requirements in the fields of aerospace, aviation, aerospace, weapons, electronics, ships, communications, etc., high-frequency circuits have increasingly stringent requirements on the ESR value of tantalum capacitors, especially with the continuous increase in the frequency of use of active filter circuits, which puts higher requirements on the ESR value parameters of capacitors. The core anode design, sintering, empowerment, coating and packaging of solid electrolytic capacitors will affect the ESR value of the capacitor, but the cathode MnO 2 The manufacturing level of the layer and the extraction efficiency of the cathode have the greatest impact on the ESR value of the capacitor. Therefore, it is necessary to find new processes, new technologies and new materials to reduce the ESR value of high-frequency products. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above background technology, the purpose of the present invention is to provide a high-capacity thin-film tantalum electrolytic capacitor and its preparation process, using graphite and polymer silver paste as cathode lead-out materials, and the polymer silver paste uses modified nano-silver powder as a conductive material. The modified nano-silver powder effectively improves the conductivity of the polymer silver paste, thereby reducing the ESR value of the capacitor.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high-capacity thin-film tantalum electrolytic capacitor comprises an anode tantalum core, one end of the anode tantalum core is fixedly connected to a positive lead at the center of the circle, the positive lead is a tantalum wire, and a Ta 2 O 5 Thin film, Ta 2 O 5A manganese dioxide layer is arranged on the outer layer of the film, a graphite layer is arranged on the outer layer of the manganese dioxide, a polymer silver paste layer is arranged on the outer layer of the graphite, the polymer silver paste layer comprises the following raw materials in parts by weight: 40-50 parts of modified nano silver powder, 5-10 parts of bisphenol A epoxy resin, 1-2 parts of curing agent, 3-5 parts of ethyl acetate, and 0.5-1 part of active diluent; the polymer silver paste layer is coated with a silver shell, the silver shell is fixedly connected to the negative electrode lead, and an open end of the silver shell close to the positive electrode lead is sealed with an insulator.

[0007] Further preferably, the modified nano silver powder is a hydrophobic nano silver powder modified by a silane coupling agent, and the preparation method thereof comprises the following steps:

[0008] (1) dissolving silver nitrate in deionized water, then adding ammonia water and stirring to mix well to prepare a silver ammonia solution;

[0009] (2) Add deionized water, polyvinyl pyrrolidone and glucose into the reaction kettle, stir and heat to 45-50°C, slowly add the silver ammonia solution dropwise into the reaction kettle, and react for 40-60 minutes;

[0010] (3) Add 20 wt% potassium hydroxide to the reactor, stir and react for 1-3 hours, let stand for 24 hours after the reaction, remove the supernatant, wash the precipitate with deionized water and ethanol for 3-5 times, add butyl carbitol (30% by weight of the silver powder), and then distill to evaporate the low-boiling point solvent. After washing with ethanol, bake at 110°C for 60 minutes to obtain nano silver powder;

[0011] (4) Add the KH-560 solution into a three-necked flask, add hydrochloric acid solution dropwise to adjust the pH value to 4, then add nano-silver powder, and ultrasonically disperse the mixed solution in a constant temperature water bath at 40°C while mechanically stirring. After a certain reaction time, filter the reactant, wash with toluene, and vacuum dry at 60°C to obtain modified nano-silver powder.

[0012] Further preferably, in step (4), the mass ratio of KH-560 to nano silver powder is 1:10-15.

[0013] More preferably, the curing agent is one of imidazoles, imidazolines, trialkylphosphine, quaternary ammonium salts, quaternary phosphonium salts and organic ureas.

[0014] Further preferably, the active diluent is one of polypropylene glycol diglycidyl ether, phenyl glycidyl ether or ethylene glycol diglycidyl ether.

[0015] A method for preparing a high-capacity thin-film tantalum electrolytic capacitor comprises the following steps:

[0016] S1. Select tantalum powder with specific capacitance corresponding to the capacitor voltage, add graphite and phenolic resin and mix evenly to form a mixed powder. Press the mixed powder and tantalum wire into a density of 5~7.5g / cm -3 Columnar, 1×10 -3 Pre-sintering at 1200-1350°C for 25-40 min under Pa vacuum conditions, then heating to 1550-1800°C for 2-4 h, then cooling to 60-80°C before breaking the vacuum to obtain a tantalum core;

[0017] S2, immerse the tantalum core in 0.1~2wt% phosphoric acid solution, connect the tantalum core to the positive electrode of the power supply, connect the energy tank to the negative electrode of the power supply, control the temperature to 80~90℃, and the current density to 15~30mA / g, and perform electrochemical treatment to form a dense Ta on the surface of the tantalum core. 2 O 5 film;

[0018] S3, immersing the tantalum core in a 1-2wt% manganese nitrate solution for 10-20 minutes, taking it out and drying it at 60-80°C, then heating it to 180-200°C for 15-30 minutes, repeating this process 3-5 times, and forming a manganese dioxide layer on the surface of the tantalum core;

[0019] S4, immersing the tantalum core in a 7-8 wt% colloidal graphite solution, drying at 130-220° C. for 20-30 min, repeating 3-5 times, to form a graphite layer outside the manganese dioxide layer;

[0020] S5. Mix the raw materials of the polymer silver paste layer in proportion to prepare a polymer silver paste, then coat the polymer silver paste on the outer wall of the graphite layer, and finally wrap the tantalum core with a silver shell, fill the gap between the silver shell and the tantalum core with the polymer silver paste, and after the polymer silver paste is completely cured, seal the opening of the silver shell with insulation.

[0021] Beneficial effects of the present invention:

[0022] The present invention uses graphite and polymer silver paste as cathode lead-out materials, and the polymer silver paste uses modified nano silver powder as a conductive material. The modified nano silver powder effectively improves the conductivity of the polymer silver paste, thereby reducing the ESR value of the capacitor. The modified nano silver powder uses glucose as a reducing agent, a silver-ammine complex as a precursor, and a PVP polymer protective agent. It is prepared in an alkaline environment medium under high temperature conditions, and the silver powder particle size is nanometer-level. The nano silver powder is surface-modified by a silane coupling agent to reduce the agglomeration of the nano silver powder, improve its dispersibility and stability, and is conducive to the nano silver powder maintaining good conductive properties during long-term use. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A modified nano silver powder, wherein the modified nano silver powder is a hydrophobic nano silver powder modified by a silane coupling agent, and the preparation method thereof comprises the following steps:

[0026] (1) dissolving silver nitrate in deionized water, adding ammonia water and stirring to mix evenly until the precipitate is dissolved to prepare a silver ammonia solution;

[0027] (2) Add deionized water, polyvinyl pyrrolidone and glucose into the reaction kettle, stir and heat to 48°C, slowly add the silver ammonia solution dropwise into the reaction kettle, and react for 50 minutes;

[0028] (3) Add 20 wt% potassium hydroxide to the reactor, stir and react for 2 h, let the reaction stand for 24 h, remove the supernatant, wash the precipitate with deionized water and ethanol for 3 to 5 times, add butyl carbitol (30% by weight of the silver powder), and then distill to evaporate the low-boiling point solvent. After washing with ethanol, bake at 110° C. for 60 min to obtain nano silver powder;

[0029] (4) Add 5 g of KH-560 solution into a three-necked flask, add hydrochloric acid solution to adjust the pH value to 4, then add nano-silver powder, and ultrasonically disperse the mixed solution in a constant temperature water bath at 40°C while mechanically stirring. After a certain reaction time, filter the reactant, wash with toluene, and vacuum dry at 60°C to obtain modified nano-silver powder.

[0030] Example 2

[0031] A high-capacity thin-film tantalum electrolytic capacitor comprises an anode tantalum core, one end of the anode tantalum core is fixedly connected to a positive lead at the center of the circle, the positive lead is a tantalum wire, and a Ta 2 O 5 Thin film, Ta 2 O 5A manganese dioxide layer is provided on the outer layer of the film, a graphite layer is provided on the outer layer of the manganese dioxide, a polymer silver paste layer is provided on the outer layer of the graphite, the polymer silver paste layer comprises the following raw materials in parts by weight: 50 parts of modified nano silver powder, 5 parts of bisphenol A epoxy resin, 2 parts of 1,1'-(4-methyl-m-phenylene)bis(3,3-dimethylurea), 3 parts of ethyl acetate, and 1 part of ethylene glycol diglycidyl ether; the polymer silver paste layer is coated with a silver shell, the silver shell is fixedly connected to the negative electrode lead, and the open end of the silver shell close to the positive electrode lead is sealed with an insulator.

[0032] The method for preparing the high-capacity thin-film tantalum electrolytic capacitor comprises the following steps:

[0033] S1. Select tantalum powder with specific capacitance corresponding to the capacitor voltage, add graphite and phenolic resin and mix evenly to form a mixed powder. Press the mixed powder and tantalum wire into a density of 5g / cm -3 Columnar, 1×10 -3 The tantalum core was pre-sintered at 1350°C for 25 min under a Pa vacuum condition, then heated to 1800°C and sintered for 2 h, and then cooled to 80°C before breaking the vacuum to obtain a tantalum core.

[0034] S2, the tantalum core is immersed in 0.1wt% phosphoric acid solution, the tantalum core is connected to the positive electrode of the power supply, the enabling tank is connected to the negative electrode of the power supply, the temperature is controlled at 90℃, the current density is 15mA / g, and electrochemical treatment is performed to form a dense Ta on the surface of the tantalum core. 2 O 5 film;

[0035] S3, immersing the tantalum core in a 2wt% manganese nitrate solution for 10 minutes, taking it out and drying it at 80°C, then heating it to 180°C for 30 minutes, repeating this process 3 to 5 times, and forming a manganese dioxide layer on the surface of the tantalum core;

[0036] S4, immersing the tantalum core in a 7wt% colloidal graphite solution, drying at 220°C for 20 minutes, repeating 3 to 5 times, to form a graphite layer outside the manganese dioxide layer;

[0037] S5. Mix the raw materials of the polymer silver paste layer in proportion to prepare a polymer silver paste, then coat the polymer silver paste on the outer wall of the graphite layer, and finally wrap the tantalum core with a silver shell, fill the gap between the silver shell and the tantalum core with the polymer silver paste, and after the polymer silver paste is completely cured, seal the opening of the silver shell with insulation.

[0038] Example 3

[0039] A high-capacity thin-film tantalum electrolytic capacitor comprises an anode tantalum core, one end of the anode tantalum core is fixedly connected to a positive lead at the center of the circle, the positive lead is a tantalum wire, and a Ta 2 O 5 Thin film, Ta 2 O 5A manganese dioxide layer is provided on the outer layer of the film, a graphite layer is provided on the outer layer of the manganese dioxide, a polymer silver paste layer is provided on the outer layer of the graphite, the polymer silver paste layer comprises the following raw materials in parts by weight: 40 parts of modified nano silver powder, 10 parts of bisphenol A epoxy resin, 1 part of tetrabutylammonium chloride, 5 parts of ethyl acetate, and 0.5 parts of phenyl glycidyl ether; the polymer silver paste layer is coated with a silver shell, the silver shell is fixedly connected to the negative electrode lead, and an open end of the silver shell close to the positive electrode lead is sealed with an insulator.

[0040] The method for preparing the high-capacity thin-film tantalum electrolytic capacitor comprises the following steps:

[0041] S1. Select tantalum powder with specific capacitance corresponding to the capacitor voltage, add graphite and phenolic resin and mix evenly to form a mixed powder. Press the mixed powder and tantalum wire into a density of 7.5g / cm -3 Columnar, 1×10 -3 The tantalum core was pre-sintered at 1200°C for 40 min under a Pa vacuum condition, then heated to 1550°C and continued sintering for 4 h, and then cooled to 60°C before breaking the vacuum to obtain a tantalum core.

[0042] S2, the tantalum core is immersed in a 2wt% phosphoric acid solution, the tantalum core is connected to the positive electrode of the power supply, the enabling tank is connected to the negative electrode of the power supply, the temperature is controlled at 80℃, the current density is 30mA / g, and electrochemical treatment is performed to form a dense Ta on the surface of the tantalum core. 2 O 5 film;

[0043] S3, immersing the tantalum core in a 1wt% manganese nitrate solution for 20 minutes, taking it out and drying it at 60°C, then heating it to 200°C for 15 minutes, repeating this process 3 to 5 times, and forming a manganese dioxide layer on the surface of the tantalum core;

[0044] S4, immersing the tantalum core in 8wt% colloidal graphite solution, drying at 130°C for 30min, repeating 3 to 5 times, to form a graphite layer outside the manganese dioxide layer;

[0045] S5. Mix the raw materials of the polymer silver paste layer in proportion to prepare a polymer silver paste, then coat the polymer silver paste on the outer wall of the graphite layer, and finally wrap the tantalum core with a silver shell, fill the gap between the silver shell and the tantalum core with the polymer silver paste, and after the polymer silver paste is completely cured, seal the opening of the silver shell with insulation.

[0046] Example 4

[0047] A high-capacity thin-film tantalum electrolytic capacitor comprises an anode tantalum core, one end of the anode tantalum core is fixedly connected to a positive lead at the center of the circle, the positive lead is a tantalum wire, and a Ta 2 O 5 Thin film, Ta 2 O 5A manganese dioxide layer is provided on the outer layer of the film, a graphite layer is provided on the outer layer of the manganese dioxide, a polymer silver paste layer is provided on the outer layer of the graphite, the polymer silver paste layer comprises the following raw materials in parts by weight: 45 parts of modified nano silver powder, 8 parts of bisphenol A epoxy resin, 1.5 parts of 2-ethyl 4-methylimidazole, 4 parts of ethyl acetate, and 0.8 parts of polypropylene glycol diglycidyl ether; the polymer silver paste layer is coated with a silver shell, the silver shell is fixedly connected to the negative electrode lead, and the open end of the silver shell close to the positive electrode lead is sealed with an insulator.

[0048] The method for preparing the high-capacity thin-film tantalum electrolytic capacitor comprises the following steps:

[0049] S1. Select tantalum powder with specific capacitance corresponding to the capacitor voltage, add graphite and phenolic resin and mix evenly to form a mixed powder. Press the mixed powder and tantalum wire into a density of 6g / cm -3 Columnar, 1×10 -3 Pre-sintering at 1280°C for 25-40 min under Pa vacuum conditions, then heating to 1650°C and continuing sintering for 3 h, then cooling to 70°C and breaking the vacuum to obtain a tantalum core;

[0050] S2, the tantalum core is immersed in 1wt% phosphoric acid solution, the tantalum core is connected to the positive electrode of the power supply, the enabling tank is connected to the negative electrode of the power supply, the temperature is controlled at 85℃, the current density is 24mA / g, and electrochemical treatment is performed to form a dense Ta on the surface of the tantalum core. 2 O 5 film;

[0051] S3, immersing the tantalum core in a 1.5wt% manganese nitrate solution for 15 minutes, taking it out and drying it at 70°C, then heating it to 190°C for 20 minutes, repeating this process 3 to 5 times, and forming a manganese dioxide layer on the surface of the tantalum core;

[0052] S4, immersing the tantalum core in a 7.5wt% colloidal graphite solution, drying at 180°C for 25min, repeating 3 to 5 times, to form a graphite layer outside the manganese dioxide layer;

[0053] S5. Mix the raw materials of the polymer silver paste layer in proportion to prepare a polymer silver paste, then coat the polymer silver paste on the outer wall of the graphite layer, and finally wrap the tantalum core with a silver shell, fill the gap between the silver shell and the tantalum core with the polymer silver paste, and after the polymer silver paste is completely cured, seal the opening of the silver shell with insulation.

[0054] Comparative Example 1

[0055] A high-capacity thin-film tantalum electrolytic capacitor comprises an anode tantalum core, one end of the anode tantalum core is fixedly connected to a positive lead at the center of the circle, the positive lead is a tantalum wire, and a Ta 2 O 5 Thin film, Ta 2 O 5A manganese dioxide layer is provided on the outer layer of the film, a graphite layer is provided on the outer layer of the manganese dioxide, a polymer silver paste layer is provided on the outer layer of the graphite, the polymer silver paste layer comprises the following raw materials in parts by weight: 45 parts of nano silver powder, 8 parts of bisphenol A epoxy resin, 1.5 parts of 2-ethyl 4-methylimidazole, 4 parts of ethyl acetate, and 0.8 parts of polypropylene glycol diglycidyl ether; the polymer silver paste layer is coated with a silver shell, the silver shell is fixedly connected to the negative electrode lead, and the open end of the silver shell close to the positive electrode lead is sealed with an insulator.

[0056] The preparation method of the above-mentioned high-capacity thin film tantalum electrolytic capacitor is the same as that of Example 4.

[0057] Performance Testing

[0058] The solid tantalum electrolytic capacitors prepared in Examples 2 to 4 and Comparative Example 1 were tested for capacity, leakage current, equivalent series resistance ESR and loss tangent at 25°C. The capacity, loss tangent and ESR tests were tested using a TH2816 wideband LCR digital bridge, and the leakage current was tested using a TH2683 leakage current tester. The measurement conditions for each parameter are as follows: the capacity and loss tangent measurement frequency is 1000Hz, the DC bias is 2.2V, and the signal level is 1Vrms; the ESR test frequency is 100KHz, the DC bias is 2V, and the signal level is 0.5Vrms; when measuring the DC leakage current at room temperature, the reading is taken after charging for 60s at 1.2 times the rated voltage, and when measuring at 125°C, a derated voltage needs to be applied for measurement. The results are shown in Table 1 below:

[0059] Table 1 Performance test results of solid tantalum electrolytic capacitors

[0060]

[0061] It can be seen from the data in the above table that the solid tantalum electrolytic capacitors prepared in Examples 2 to 4 of the present invention have lower leakage current and equivalent series resistance than those in Comparative Example 1, and the loss is also lower than that in Comparative Example 1.

[0062] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0063] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A method for preparing modified nano silver powder, characterized in that: The modified nano silver powder is a hydrophobic nano silver powder modified by a silane coupling agent, and the preparation method thereof comprises the following steps: (1) dissolving silver nitrate in deionized water, then adding ammonia water and stirring to mix well to prepare a silver ammonia solution; (2) Add deionized water, polyvinyl pyrrolidone and glucose into the reaction kettle, stir and heat to 45-50°C, slowly add the silver ammonia solution dropwise into the reaction kettle, and react for 40-60 minutes; (3) Add 20 wt% potassium hydroxide to the reactor, stir and react for 1-3 hours, let stand for 24 hours after the reaction, remove the supernatant, wash the precipitate with deionized water and ethanol for 3-5 times, add butyl carbitol (30% by weight of the silver powder), and then distill to evaporate the low-boiling point solvent. After washing with ethanol, bake at 110°C for 60 minutes to obtain nano silver powder; (4) Add KH-560 solution into a three-necked flask, add hydrochloric acid solution to adjust the pH value to 4, and then add nano-silver powder. The mass ratio of KH-560 to nano-silver powder is 1:10-15. The mixed solution is ultrasonically dispersed in a 40°C constant temperature water bath while being mechanically stirred. After a certain reaction time, the reactant is filtered, washed with toluene, and vacuum dried at 60°C to obtain modified nano-silver powder.

2. A high capacity thin film tantalum electrolytic capacitor, characterized in that: The invention comprises an anode tantalum core, wherein the center of one end of the anode tantalum core is fixedly connected to a positive lead, the positive lead is a tantalum wire, a Ta2O5 film is provided on the surface of the anode tantalum core, a manganese dioxide layer is provided on the outer layer of the Ta2O5 film, a graphite layer is provided on the outer layer of the manganese dioxide layer, a polymer silver paste layer is provided on the outer layer of the graphite layer, the polymer silver paste layer comprises the following raw materials in parts by weight: 40-50 parts of hydrophobic nano silver powder modified by a silane coupling agent prepared according to the preparation method of modified nano silver powder according to claim 1, 5-10 parts of bisphenol A epoxy resin, 1-2 parts of curing agent, 3-5 parts of ethyl acetate, and 0.5-1 part of active diluent, the polymer silver paste layer is coated with a silver shell, the silver shell is fixedly connected to a negative lead, and the silver shell is sealed with an insulator at an open end near one end of the positive lead.

3. The high-capacity thin-film tantalum electrolytic capacitor according to claim 2, characterized in that: The curing agent is one of imidazoles, imidazolines, trialkylphosphine, quaternary ammonium salts, quaternary phosphonium salts and organic ureas.

4. The high-capacity thin-film tantalum electrolytic capacitor according to claim 2, characterized in that: The active diluent is one of polypropylene glycol diglycidyl ether, phenyl glycidyl ether or ethylene glycol diglycidyl ether.

5. The process for preparing a high-capacity thin-film tantalum electrolytic capacitor according to any one of claims 2 to 4, characterized in that: The following steps are involved: S1. Select tantalum powder with specific capacitance corresponding to the capacitor voltage, add graphite and phenolic resin and mix evenly to form a mixed powder. Press the mixed powder and tantalum wire into a density of 5~7.5g / cm -3 Columnar, 1×10 -3 Pre-sintering at 1200-1350°C for 25-40 min under Pa vacuum conditions, then heating to 1550-1800°C for 2-4 h, then cooling to 60-80°C before breaking the vacuum to obtain a tantalum core; S2, immerse the tantalum core in a 0.1~2wt% phosphoric acid solution, connect the tantalum core to the positive electrode of the power supply, connect the enabling tank to the negative electrode of the power supply, control the temperature to 80~90℃, and the current density to 15~30mA / g, perform electrochemical treatment, and form a dense Ta2O5 film on the surface of the tantalum core; S3, immersing the tantalum core in a 1-2wt% manganese nitrate solution for 10-20 minutes, taking it out and drying it at 60-80°C, then heating it to 180-200°C for 15-30 minutes, repeating this process 3-5 times, and forming a manganese dioxide layer on the surface of the tantalum core; S4, immersing the tantalum core in a 7-8 wt% colloidal graphite solution, drying at 130-220° C. for 20-30 min, repeating 3-5 times, to form a graphite layer outside the manganese dioxide layer; S5. Mix the raw materials of the polymer silver paste layer in proportion to prepare a polymer silver paste, then coat the polymer silver paste on the outer wall of the graphite layer, and finally wrap the tantalum core with a silver shell, fill the gap between the silver shell and the tantalum core with the polymer silver paste, and after the polymer silver paste is completely cured, seal the opening of the silver shell with insulation.

Citation Information

Patent Citations

  • Polymer chip tantalum capacitor silver paste and preparation method thereof

    CN116013576A

  • Ultrahigh-voltage and high-reliability chip tantalum capacitor and manufacturing method thereof

    CN117711825A